PA66 30% Carbon Fiber Material Data Sheet

PA66 30% Carbon Fiber (Polyamide 66) Material Data Sheet

PA66 30% Carbon Fiber Overview

PA66 30% carbon fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 30% PAN Carbon Fiber, Conductive – EMI Shielding). This PA66 30% carbon fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 30% Carbon Fiber Designation

Polyamide (Nylon) (Type 66, 30% PAN Carbon Fiber, Conductive – EMI Shielding)
TradenamesBestnyl, LNP Thermocomp, Luvocom, Novamid, Nylfor, Staramide, Star-Therm, Strator, Tecomid, Tribocomp, Wellamid

PA66 30% Carbon Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 30% Carbon Fiber Composition detail

Polymer70  %
Carbon (fiber)30  %

PA66 30% Carbon Fiber Physical properties

Density1.27–1.29g/cm3

PA66 30% Carbon Fiber Mechanical properties

Young’s modulus17.8–22.2GPa
Specific stiffness13.9–17.3MN.m/kg
Yield strength (elastic limit)178–222MPa
Tensile strength180–220MPa
Specific strength139–173kN.m/kg
Elongation2.46–3.54% strain
Elongation at yield2.07–3.93% strain
Compressive modulus19–21GPa
Compressive strength228–252MPa
Flexural modulus13.1–15.7GPa
Flexural strength (modulus of rupture)203–248MPa
Shear modulus7.34–7.72GPa
Shear strength108–132MPa
Bulk modulus18.4–20.3GPa
Poisson’s ratio0.315–0.328 
Shape factor8.19
Hardness – Vickers57–63HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)788–1250kJ/m3
Fatigue strength at 10^7 cycles76–84MPa

PA66 30% Carbon Fiber Impact & fracture properties

Fracture toughness5.6–6.19MPa.m0.5
Toughness (G)1.51–2.01kJ/m2
Impact strength, notched 23 °C12.5–24.2kJ/m2
Impact strength, notched -30 °C8.85–19.2kJ/m2
Impact strength, unnotched 23 °C47.1–69.2kJ/m2

PA66 30% Carbon Fiber Thermal properties

Melting point258–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa260–266°C
Heat deflection temperature 1.8MPa243–260°C
Maximum service temperature90–130°C
Minimum service temperature-81–-71°C
Thermal conductivity0.97–1.05W/m.°C
Specific heat capacity1410–1470J/kg.°C
Thermal expansion coefficient19.8–28.8µstrain/°C
Thermal shock resistance331–529°C
Thermal distortion resistance0.0349–0.0511MW/m

PA66 30% Carbon Fiber Electrical properties

Electrical resistivity2e9–5e10µohm.cm
Electrical conductivity3.45e-9–8.62e-8%IACS
Comparative tracking index100  V
Galvanic potential0.14–0.22V

PA66 30% Carbon Fiber Magnetic properties

Magnetic typeNon-magnetic

PA66 30% Carbon Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3720–4170m/s
Mechanical loss coefficient (tan delta)0.00662–0.00732 

PA66 30% Carbon Fiber Absorption & permeability

Water absorption @ 24 hrs0.51–0.83%
Water absorption @ sat5–6.6%
Humidity absorption @ sat1.4–1.8%

PA66 30% Carbon Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionUnsuitable
Polymer thermoformingLimited use
Linear mold shrinkage0.1 – 0.3 %
Melt temperature220 – 310 °C
Mold temperature60 – 80 °C
Molding pressure range68.8 – 138 MPa

PA66 30% Carbon Fiber Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning