PA66 30% Long Carbon Fiber (Polyamide 66) Material Data Sheet
PA66 30% Long Carbon Fiber Overview
PA66 30% long carbon fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 30% Long Carbon Fiber). This PA66 30% long carbon fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.
PA66 30% Long Carbon Fiber Designation
Polyamide (Nylon) (Type 66, 30% Long Carbon Fiber)
Tradenames
Complet, Edgetek, Onforce, Strator, Witcom
PA66 30% Long Carbon Fiber Typical uses
Automotive applications, structural parts
PA66 30% Long Carbon Fiber Composition detail
Polymer
70
%
Carbon (fiber)
30
%
PA66 30% Long Carbon Fiber Physical properties
Density
1.26
–
1.3
g/cm3
PA66 30% Long Carbon Fiber Mechanical properties
Young’s modulus
23
–
24
GPa
Specific stiffness
17.9
–
18.8
MN.m/kg
Yield strength (elastic limit)
276
–
330
MPa
Tensile strength
286
–
350
MPa
Specific strength
215
–
258
kN.m/kg
Elongation
1
–
2
% strain
Compressive modulus
13.8
–
14.4
GPa
Compressive strength
352
–
410
MPa
Flexural modulus
18
–
22.5
GPa
Flexural strength (modulus of rupture)
380
–
450
MPa
Shear modulus
8.67
–
9.11
GPa
Shear strength
176
–
205
MPa
Bulk modulus
22.9
–
24.1
GPa
Poisson’s ratio
0.315
–
0.328
Shape factor
6.9
Hardness – Vickers
70
–
77
HV
Hardness – Shore D
104
–
114
Elastic stored energy (springs)
1630
–
2300
kJ/m3
Fatigue strength at 10^7 cycles
80.2
–
93.6
MPa
PA66 30% Long Carbon Fiber Impact & fracture properties
Fracture toughness
14.6
–
17.7
MPa.m0.5
Toughness (G)
9.16
–
13.2
kJ/m2
Impact strength, notched 23 °C
15
–
19
kJ/m2
Impact strength, notched -30 °C
12.7
–
15.4
kJ/m2
Impact strength, unnotched 23 °C
55
–
100
kJ/m2
PA66 30% Long Carbon Fiber Thermal properties
Melting point
242
–
282
°C
Glass temperature
54
–
66
°C
Heat deflection temperature 0.45MPa
255
°C
Heat deflection temperature 1.8MPa
249
–
252
°C
Vicat softening point
240
–
255
°C
Maximum service temperature
107
–
127
°C
Minimum service temperature
-81
–
-71
°C
Thermal conductivity
0.989
–
1.03
W/m.°C
Specific heat capacity
1410
–
1470
J/kg.°C
Thermal expansion coefficient
6
µstrain/°C
Thermal shock resistance
1950
–
2350
°C
Thermal distortion resistance
0.165
–
0.172
MW/m
PA66 30% Long Carbon Fiber Electrical properties
Electrical resistivity
2e9
–
5e10
µohm.cm
Electrical conductivity
3.45e-9
–
8.62e-8
%IACS
Galvanic potential
0.14
–
0.22
V
PA66 30% Long Carbon Fiber Magnetic properties
Magnetic type
Non-magnetic
PA66 30% Long Carbon Fiber Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
4230
–
4340
m/s
Mechanical loss coefficient (tan delta)
0.00475
–
0.00628
PA66 30% Long Carbon Fiber Absorption & permeability