PEKK 30% Carbon Fiber Material Data Sheet

PEKK 30% Carbon Fiber (Polyetherketoneketone) Material Data Sheet

PEKK 30% Carbon Fiber Overview

PEKK 30% carbon fiber is a grade of polyetherketoneketone (PEKK), designated Polyetherketoneketone (30% carbon fiber). This PEKK 30% carbon fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PEKK parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PEKK parts in-house and inspects them before shipment.

PEKK Designation

Polyetherketoneketone (30% carbon fiber)
TradenamesOxpekk

PEKK 30% Carbon Fiber Composition detail

Polymer70  %
Carbon (fiber)30  %

PEKK Physical properties

Density1.35–1.37g/cm3

PEKK 30% Carbon Fiber Mechanical properties

Young’s modulus27.5–28.1GPa
Specific stiffness20.2–20.7MN.m/kg
Yield strength (elastic limit)189–209MPa
Tensile strength236–260MPa
Specific strength139–154kN.m/kg
Elongation1.11–1.29% strain
Elongation at yield1.1–1.3% strain
Compressive modulus27.5–28.1GPa
Flexural modulus21.6–24.4GPa
Flexural strength (modulus of rupture)376–396MPa
Shear modulus10–11GPa
Shear strength108–119MPa
Poisson’s ratio0.42–0.46 
Shape factor10.3
Hardness – Vickers56–62HV
Elastic stored energy (springs)644–784kJ/m3
Fatigue strength at 10^7 cycles94.2–104MPa

PEKK Impact & fracture properties

Impact strength, notched 23 °C5.04–6.16kJ/m2
Impact strength, unnotched 23 °C53–56kJ/m2

PEKK 30% Carbon Fiber Thermal properties

Melting point347–373°C
Glass temperature153–170°C
Heat deflection temperature 0.45MPa317–341°C
Heat deflection temperature 1.8MPa309–333°C
Vicat softening point317–341°C
Maximum service temperature233–287°C
Specific heat capacity1460–1490J/kg.°C
Thermal expansion coefficient9.75–10.3µstrain/°C
Thermal shock resistance676–757°C

PEKK Electrical properties

Electrical resistivity9250000000000000–10800000000000000µohm.cm
Electrical conductivity1.6e-14–1.86e-14%IACS
Dielectric constant (relative permittivity)3.17–3.43 
Dissipation factor (dielectric loss tangent)0.0035–0.0045 
Dielectric strength (dielectric breakdown)23–25MV/m
Galvanic potential0.14–0.22V

PEKK Magnetic properties

Magnetic typeNon-magnetic

PEKK Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity4490–4550m/s

PEKK Absorption & permeability

Water absorption @ 24 hrs0.09–0.11%

PEKK Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingUnsuitable
Linear mold shrinkage0.08 – 0.12 %

PEKK Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oils and fuelsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Excellent
FlammabilitySelf-extinguishing