Cast High Conductivity Copper Material Data Sheet

High Conductivity Copper Material Data Sheet (Cast)

Cast High Conductivity Copper Overview

Cast high conductivity copper is a cast high conductivity copper, known as h.c. copper. Condition: Cast. This cast high conductivity copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for high conductivity copper castings from Turkey (Türkiye)? Modulus Metal supplies high conductivity copper castings with in-house CNC machining and inspects them before shipment.

H.C. Copper Designation

Copper Alloy: hc-Cu

H.C. Copper Typical uses

Castings, electrical components, fittings for liquid gases.

Cast High Conductivity Copper Composition detail

C (carbon)0–0.1%
Cu (copper)99.9–100%

H.C. Copper Physical properties

Density8.94–8.95g/cm3

Cast High Conductivity Copper Mechanical properties

Young’s modulus122–128GPa
Specific stiffness13.6–14.3MN.m/kg
Yield strength (elastic limit)28–40MPa
Tensile strength145–160MPa
Specific strength3.13–4.47kN.m/kg
Elongation23–25% strain
Compressive strength28–40MPa
Flexural modulus122–128GPa
Flexural strength (modulus of rupture)28–40MPa
Shear modulus45.1–47.4GPa
Bulk modulus132–138GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers43–46HV
Elastic stored energy (springs)3.22–6.23kJ/m3
Fatigue strength at 10^7 cycles91–97MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
84.9–104MPa

H.C. Copper Impact & fracture properties

Fracture toughness100–107MPa.m0.5
Toughness (G)79.8–91.4kJ/m2

Cast High Conductivity Copper Thermal properties

Melting point1080  °C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity390–398W/m.°C
Specific heat capacity383–387J/kg.°C
Thermal expansion coefficient16.8–16.9µstrain/°C
Thermal shock resistance13.3–19°C
Thermal distortion resistance23.1–23.6MW/m
Latent heat of fusion200–208kJ/kg

H.C. Copper Electrical properties

Electrical resistivity1.91–1.95µohm.cm
Electrical conductivity88.4–90.3%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

H.C. Copper Magnetic properties

Magnetic typeNon-magnetic

H.C. Copper Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3690–3780m/s
Mechanical loss coefficient (tan delta)0.0025–0.0051 

H.C. Copper Processing properties

Metal castingLimited use
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed29.3 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

H.C. Copper Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

Cast High Conductivity Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

H.C. Copper Notes

Cast High Conductivity Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

H.C. Copper Standards with similar compositions

Japan: CAC101 to JIS H5120, CAC102 to JIS H5120, CAC103 to JIS H5120
USA: C81200, UNS C80300, UNS C80500, UNS C80700, UNS C80900, UNS C81200
Tradenames: LEADED GUN METAL, PHOSPHOR COPPER GRADE B