Home » High Conductivity Copper » C14700 H.C. Copper, Hard Material Data Sheet
C14700 H.C. Copper Material Data Sheet (Wrought, Hard)
C14700 Hard Copper Overview
C14700 hard copper is a wrought high conductivity copper (UNS C14700, EN CW114C), known as h.c. copper. Condition: Hard. This C14700 hard copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14700 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14700 copper parts in-house and inspects them before shipment.
C14700 Designation
Wrought Copper Alloy: hc-CuS(h); C111 (UNS C14700) Condition Hard UNS number C14700 EN name CW114C ISO name CuS(P0,03)
C14700 Hard Copper Composition detail
Cu (copper) 99.5 – 99.8 % P (phosphorus) 0.002 – 0.005 % S (sulfur) 0.2 – 0.5 %
C14700 Physical properties
C14700 Hard Copper Mechanical properties
Young’s modulus 128 – 135 GPa Specific stiffness 14.3 – 15.1 MN.m/kg Yield strength (elastic limit) 230 – 320 MPa Tensile strength 270 – 350 MPa Specific strength 25.7 – 35.8 kN.m/kg Elongation 5 – 15 % strain Compressive strength 230 – 320 MPa Flexural modulus 128 – 135 GPa Flexural strength (modulus of rupture) 230 – 320 MPa Shear modulus 45 – 50 GPa Bulk modulus 138 – 146 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 27 Hardness – Vickers 85 – 110 HV Elastic stored energy (springs) 206 – 381 kJ/m3 Fatigue strength at 10^7 cycles 90 – 105 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 75 – 126 MPa
C14700 Impact & fracture properties
Fracture toughness 40.4 – 50 MPa.m0.5 Toughness (G) 12.5 – 18.8 kJ/m2
C14700 Hard Copper Thermal properties
Melting point 1070 – 1080 °C Maximum service temperature 77 – 87 °C Minimum service temperature -273 °C Thermal conductivity 365 – 370 W/m.°C Specific heat capacity 377 – 383 J/kg.°C Thermal expansion coefficient 17 – 18 µstrain/°C Thermal shock resistance 99.7 – 140 °C Thermal distortion resistance 20.4 – 21.6 MW/m Latent heat of fusion 200 – 208 kJ/kg
C14700 Electrical properties
Electrical resistivity 1.82 – 1.86 µohm.cm Electrical conductivity 92.7 – 94.7 %IACS Temperature dependence of resistivity 5.2 – 5.4 /°C Galvanic potential -0.2 – -0.12 V
C14700 Magnetic properties
Magnetic type Non-magnetic
C14700 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3780 – 3890 m/s Mechanical loss coefficient (tan delta) 3.9e-5 – 7.6e-5
C14700 Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Excellent Metal press forming Excellent Metal deep drawing Limited use Machining speed 29 m/min Weldability Notes: Preheating and post weld heat treatment are not required Poor
C14700 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
C14700 Hard Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Not susceptible
C14700 Notes
C14700 Hard Copper Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C14700 Standards with similar compositions
Australia: 147 to AS 1567, C14700 to AS 2738Europe: CW114C to CEN EN 12164, CW114C to CEN EN 12168Germany: 2.1498 to DIN, CuSP to DINInternational: CuS(P0.01) to ISO 1637, CuS(P0.01) to ISO R1336, CuS(P0.03) to ISO 1637, CuS(P0.03) to ISO R1336UK: C111 to BS 2874USA: C14700, C14700 to ASTM B124M, C14700 to ASTM B283, C14700 to ASTM B301/B301M, C14700 to SAE J463, UNS C14700, UNS C14720Tradenames: AMSULF, BOLTOMET 917, BRIDGEPORT NO. 120, ERM CUS, MCKECHNIE SC, MUELLER 1470, MUELLER 1476, OFHC SULFUR COPPER, OSNA CU58S, SCOVILL NO. 1032, SULPH-COPPER