C14200 Tough-Pitch Arsenical H.C. Copper, Hard Material Data Sheet
C14200 Tough-Pitch Arsenical H.C. Copper Material Data Sheet (Wrought, Hard)
C14200 Hard Tough-Pitch Arsenical Overview
C14200 hard tough-pitch arsenical is a wrought general purpose copper (UNS C14200, EN CW117C, C107), known as tough-pitch arsenical h.c. copper. Condition: Hard. This C14200 hard tough-pitch arsenical material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14200 copper parts in-house and inspects them before shipment.
General engineering, electrical items of lower conductivity.
C14200 Hard Tough-Pitch Arsenical Composition detail
As (arsenic)
0.3
–
0.5
%
Cu (copper)
99.5
–
99.7
%
O2 (oxygen gas)
0.05
%
C14200 Physical properties
Density
8.94
–
8.95
g/cm3
C14200 Hard Tough-Pitch Arsenical Mechanical properties
Young’s modulus
122
–
128
GPa
Specific stiffness
13.6
–
14.3
MN.m/kg
Yield strength (elastic limit)
240
–
350
MPa
Tensile strength
310
–
400
MPa
Specific strength
26.8
–
39.1
kN.m/kg
Elongation
4
–
20
% strain
Compressive strength
240
–
350
MPa
Flexural modulus
122
–
128
GPa
Flexural strength (modulus of rupture)
240
–
350
MPa
Shear modulus
45.1
–
47.4
GPa
Bulk modulus
132
–
138
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
26
Hardness – Vickers
80
–
115
HV
Elastic stored energy (springs)
237
–
476
kJ/m3
Fatigue strength at 10^7 cycles
100
–
110
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
81
–
136
MPa
C14200 Impact & fracture properties
Fracture toughness
38
–
48.7
MPa.m0.5
Toughness (G)
11.7
–
18.7
kJ/m2
C14200 Hard Tough-Pitch Arsenical Thermal properties
Melting point
1080
°C
Maximum service temperature
120
–
130
°C
Minimum service temperature
-273
°C
Thermal conductivity
170
–
190
W/m.°C
Specific heat capacity
383
–
387
J/kg.°C
Thermal expansion coefficient
16.8
–
16.9
µstrain/°C
Thermal shock resistance
114
–
166
°C
Thermal distortion resistance
10.1
–
11.3
MW/m
Latent heat of fusion
200
–
208
kJ/kg
C14200 Electrical properties
Electrical resistivity
3.98
–
5.01
µohm.cm
Electrical conductivity
34.4
–
43.3
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
C14200 Magnetic properties
Magnetic type
Non-magnetic
C14200 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3690
–
3780
m/s
Mechanical loss coefficient (tan delta)
3.3e-5
–
6.9e-5
C14200 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
54.9 m/min
Weldability Notes: Preheating and post weld heat treatment are not required, and contains hazardous elements
Good
C14200 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
C14200 Hard Tough-Pitch Arsenical Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C14200 Notes
C14200 Hard Tough-Pitch Arsenical Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C14200 Standards with similar compositions
International: CuAs(P) to ISO 1635, CuAs(P) to ISO 1637, CuAs(P) to ISO 1640
Switzerland: Cu-DPA to VSM 11557/1
USA: C14200, C14200 to ASTM B111M, C14200 to ASTM B152M, C14200 to ASTM B359M, C14200 to ASTM B379, C14200 to ASTM B395M, C14200 to ASTM B447, C14200 to ASTM B75M, UNS C14100, UNS C14200, UNS C14210