C14200 Tough-Pitch Arsenical H.C. Copper, Soft Material Data Sheet

C14200 Tough-Pitch Arsenical H.C. Copper Material Data Sheet (Wrought, Soft)

C14200 Soft Tough-Pitch Arsenical Overview

C14200 soft tough-pitch arsenical is a wrought general purpose copper (UNS C14200, EN CW117C, C107), known as tough-pitch arsenical h.c. copper. Condition: Soft. This C14200 soft tough-pitch arsenical material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14200 copper parts in-house and inspects them before shipment.

C14200 Designation

Wrought Copper Alloy: gp-AsCu(s); C105 (UNS C14200)
ConditionSoft
UNS numberC14200
EN nameCW117C, C107
ISO nameCuSn0,15

C14200 Typical uses

General engineering, electrical items of lower conductivity.

C14200 Soft Tough-Pitch Arsenical Composition detail

As (arsenic)0.3–0.5%
Cu (copper)99.5–99.7%
O2 (oxygen gas)0.05  %

C14200 Physical properties

Density8.94–8.95g/cm3

C14200 Soft Tough-Pitch Arsenical Mechanical properties

Young’s modulus122–128GPa
Specific stiffness13.6–14.3MN.m/kg
Yield strength (elastic limit)50–70MPa
Tensile strength220–280MPa
Specific strength5.59–7.83kN.m/kg
Elongation27–50% strain
Compressive strength50–70MPa
Flexural modulus122–128GPa
Flexural strength (modulus of rupture)50–70MPa
Shear modulus45.1–47.4GPa
Bulk modulus132–138GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers40–60HV
Elastic stored energy (springs)10.2–19.1kJ/m3
Fatigue strength at 10^7 cycles80–90MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
65.8–110MPa

C14200 Impact & fracture properties

Fracture toughness86.4–95MPa.m0.5
Toughness (G)59.7–72.3kJ/m2

C14200 Soft Tough-Pitch Arsenical Thermal properties

Melting point1080  °C
Maximum service temperature120–130°C
Minimum service temperature-273  °C
Thermal conductivity170–190W/m.°C
Specific heat capacity383–387J/kg.°C
Thermal expansion coefficient16.8–16.9µstrain/°C
Thermal shock resistance23.7–33.3°C
Thermal distortion resistance10.1–11.3MW/m
Latent heat of fusion200–208kJ/kg

C14200 Electrical properties

Electrical resistivity3.98–5.01µohm.cm
Electrical conductivity34.4–43.3%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C14200 Magnetic properties

Magnetic typeNon-magnetic

C14200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3690–3780m/s
Mechanical loss coefficient (tan delta)8.16e-4–0.0016 

C14200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed54.9 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required, and contains hazardous elements
Good

C14200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C14200 Soft Tough-Pitch Arsenical Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C14200 Notes

C14200 Soft Tough-Pitch Arsenical Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C14200 Standards with similar compositions

International: CuAs(P) to ISO 1635, CuAs(P) to ISO 1637, CuAs(P) to ISO 1640
Switzerland: Cu-DPA to VSM 11557/1
USA: C14200, C14200 to ASTM B111M, C14200 to ASTM B152M, C14200 to ASTM B359M, C14200 to ASTM B379, C14200 to ASTM B395M, C14200 to ASTM B447, C14200 to ASTM B75M, UNS C14100, UNS C14200, UNS C14210
Tradenames: ARSENICAL COPPER, BRIDGEPORT NO. 108, IMI 146, NORANDA-113, PHOSPHORIZED ARSENICAL COPPER-142, REVERE ALLOY NO. 99, REVERE NO. 142, WOLVERINE ALLOY 02