C12200 Phosphorus De-Oxidized Arsenical H.C. Copper, Hard Material Data Sheet

C12200 Phosphorus De-Oxidized Arsenical H.C. Copper Material Data Sheet (Wrought, Hard)

C12200 Hard Copper Overview

C12200 hard copper is a wrought general purpose copper (UNS C12200, EN CW024A), known as phosphorus de-oxidized arsenical h.c. copper. Condition: Hard. This C12200 hard copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C12200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C12200 copper parts in-house and inspects them before shipment.

C12200 Designation

Wrought Copper Alloy: gp-Cu-DHP(h); C106 (UNS C12200)
ConditionHard
UNS numberC12200
EN nameCW024A
ISO nameCu-DHP
GB (Chinese) nameTP2
JIS (Japanese) nameC1220 / C1221

C12200 Typical uses

Hot & cold water pipes, storage tanks, heat exchangers, automobile radiators, stills, vats, anodes for electroplating & electroforming.

C12200 Hard Copper Composition detail

Cu (copper)100  %
P (phosphorus)0.015–0.04%

C12200 Physical properties

Density8.94–8.95g/cm3

C12200 Hard Copper Mechanical properties

Young’s modulus125–135GPa
Specific stiffness14–15.1MN.m/kg
Yield strength (elastic limit)185–340MPa
Tensile strength270–380MPa
Specific strength20.7–38kN.m/kg
Elongation6–25% strain
Compressive strength185–340MPa
Flexural modulus125–135GPa
Flexural strength (modulus of rupture)185–340MPa
Shear modulus45–50GPa
Bulk modulus135–146GPa
Poisson’s ratio0.34–0.35 
Shape factor27
Hardness – Vickers80–115HV
Elastic stored energy (springs)141–415kJ/m3
Fatigue strength at 10^7 cycles130–140MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
96.8–188MPa

C12200 Impact & fracture properties

Fracture toughness38.8–56.7MPa.m0.5
Toughness (G)11.9–24kJ/m2

C12200 Hard Copper Thermal properties

Melting point1080  °C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity290–360W/m.°C
Specific heat capacity378–381J/kg.°C
Thermal expansion coefficient16.8–17µstrain/°C
Thermal shock resistance84.1–155°C
Thermal distortion resistance17.2–21.3MW/m
Latent heat of fusion200–208kJ/kg

C12200 Electrical properties

Electrical resistivity1.91–2.45µohm.cm
Electrical conductivity70.4–90.3%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C12200 Magnetic properties

Magnetic typeNon-magnetic

C12200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3740–3890m/s
Mechanical loss coefficient (tan delta)3.5e-5–1.17e-4 

C12200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed28.7 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Excellent

C12200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C12200 Hard Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C12200 Notes

C12200 Hard Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C12200 Standards with similar compositions

Australia: 122 to AS 1567, C12200 to AS 2738, Cu-DHP to AS 2738, Cu-DLP to AS 2738
Canada: Cu-DHP(122) to CSA HC.4.1
Denmark: 5015 to DS 3003
Europe: CW023A to CEN EN 12163, CW023A to CEN EN 12167, CW023A to CEN EN 1653, CW024A to CEN EN 1172, CW024A to CEN EN 12163, CW024A to CEN EN 12165, CW024A to CEN EN 12166, CW024A to CEN EN 12167, CW024A to CEN EN 12420, CW024A to CEN EN 12449, CW024A to CEN EN 12450, CW024A to CEN EN 12451, CW024A to CEN EN 12452, CW024A to CEN EN 1653
Finland: Cu-DHP to SFS 2907
International: CuAs(P) to ISO 1634, Cu-DHP to ISO 1635, Cu-DHP to ISO 1637
Japan: C1201 BD to JIS H3250, C1201 BE to JIS H3250, C1201 CB/CC to JIS H2123, C1201 P/R to JIS H3100, C1201 T to JIS H3300, C1201 W to JIS H3260, C1220 BD to JIS H3250, C1220 BE to JIS H3250, C1220 CB/CC to JIS H2123, C1220 P/R to JIS H3100, C1220 T to JIS H3300, C1220 TW to JIS H3320, C1220 W to JIS H3260, C1221 P/R to JIS H3100, C1221 to JIS H3100, Cu-DHP to JIS H3401
Mexico: DHP to DGN W-23, RR to NOM W-17, RRR to NOM W-17
Norway: 16015 to NS 16015
Switzerland: Cu-DHP to VSM 11557/1
USA: BCu-1 to AWS A5.8, C10800, C10800 to ASTM B111M, C10800 to ASTM B152M, C10800 to ASTM B187M, C10800 to ASTM B359M, C10800 to ASTM B360, C10800 to ASTM B379, C10800 to ASTM B395M, C10800 to ASTM B42, C10800 to ASTM B447, C10800 to ASTM B543M, C10800 to ASTM B640, C10800 to ASTM B68M, C10800 to ASTM B743, C10800 to ASTM B75M, C12000, C12000 to ASTM B111M, C12000 to ASTM B152M, C12000 to ASTM B187M, C12000 to ASTM B359M, C12000 to ASTM B360, C12000 to ASTM B372, C12000 to ASTM B379, C12000 to ASTM B395M, C12000 to ASTM B42, C12000 to ASTM B447, C12000 to ASTM B640, C12000 to ASTM B68M, C12000 to ASTM B743, C12000 to ASTM B75M, C12000 to SAE J463, C12200, C12200 to ASTM B111M, C12200 to ASTM B152M, C12200 to ASTM B187M, C12200 to ASTM B280, C12200 to ASTM B302, C12200 to ASTM B306, C12200 to ASTM B359M, C12200 to ASTM B360, C12200 to ASTM B395M, C12200 to ASTM B447, C12200 to ASTM B543M, C12200 to ASTM B640, C12200 to ASTM B68M, C12200 to ASTM B743, C12200 to ASTM B75M, C12200 to ASTM B819, C12200 to ASTM B837, C12200 to ASTM B88, C12200 to SAE J463, C12210, C12220, C12300, C12300 to ASTM B152M, C14180, UNS C10800, UNS C12000, UNS C12200, UNS C12210, UNS C12220, UNS C12300, UNS C14180
Tradenames: 1220, AMAX LP, AMPHOS, ANACONDA 122, BOLTOMET 123, BOLTOMET 160, BOLTOMET 162, BRIDGEPORT NO. 105, BRIDGEPORT NO. 110, COPPER, DEOXIDIZED, DHP, DEOXIDIZED COPPER, DEOXIDIZED COPPER 105, DHP COPPER, DLP COPPER, MCKECHNIE DO, MUELLER 1220, OLIN C12000, OLIN COPPER 122 DHP, OUTOKUMPU K1, OUTOKUMPU K2, PHOSPHORUS-DEOXIDIZED COPPER, REVERE NO. 122, REVERE PHOSPHORUS DEOXIDIZED COPPER, SILVER COPPER, WESTERN ALLOY NO. 52, WESTERN ALLOY NO. 55, WESTERN DEOXIDIZED COPPER #52, WIELAND-K20, WIELAND-K21, WOLVERINE ALLOY 01