C12500 Fire-Refined Tough-Pitch H.C. Copper, Hard Material Data Sheet

C12500 Fire-Refined Tough-Pitch H.C. Copper Material Data Sheet (Wrought, Hard)

C12500 Hard Copper Overview

C12500 hard copper is a wrought general purpose copper (UNS C12500, EN CW006A), known as fire-refined tough-pitch h.c. copper. Condition: Hard. This C12500 hard copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C12500 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C12500 copper parts in-house and inspects them before shipment.

C12500 Designation

Wrought Copper Alloy: gp-Cu-FRTP(h); C104 (UNS C12500)
ConditionHard
UNS numberC12500
EN nameCW006A
ISO nameCu-FRTP
GB (Chinese) nameT 3

C12500 Typical uses

Architectural uses, kettles, stills, vats, gaskets, general electrical uses.

C12500 Hard Copper Composition detail

As (arsenic)0–0.012%
Bi (bismuth)0–0.003%
Cu (copper)99.9–100%
Ni (nickel)0–0.05%
Pb (lead)0–0.004%
Sb (antimony)0–0.003%
Se (selenium)0–0.0125%
Te (tellurium)0–0.0125%

C12500 Physical properties

Density8.94–8.95g/cm3

C12500 Hard Copper Mechanical properties

Young’s modulus125–135GPa
Specific stiffness14–15.1MN.m/kg
Yield strength (elastic limit)200–340MPa
Tensile strength270–380MPa
Specific strength22.4–38kN.m/kg
Elongation6–25% strain
Compressive strength200–340MPa
Flexural modulus125–135GPa
Flexural strength (modulus of rupture)200–340MPa
Shear modulus45–50GPa
Bulk modulus135–146GPa
Poisson’s ratio0.34–0.35 
Shape factor27
Hardness – Vickers80–115HV
Elastic stored energy (springs)163–421kJ/m3
Fatigue strength at 10^7 cycles95–110MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
73.1–143MPa

C12500 Impact & fracture properties

Fracture toughness38.8–54.3MPa.m0.5
Toughness (G)11.9–22.2kJ/m2

C12500 Hard Copper Thermal properties

Melting point1080  °C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity331–372W/m.°C
Specific heat capacity379–382J/kg.°C
Thermal expansion coefficient16.8–16.9µstrain/°C
Thermal shock resistance91.2–156°C
Thermal distortion resistance19.6–22.1MW/m
Latent heat of fusion200–208kJ/kg

C12500 Electrical properties

Electrical resistivity1.82–2µohm.cm
Electrical conductivity86.2–94.7%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C12500 Magnetic properties

Magnetic typeNon-magnetic

C12500 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3740–3890m/s
Mechanical loss coefficient (tan delta)3.5e-5–1e-4 

C12500 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed30.5 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

C12500 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C12500 Hard Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C12500 Notes

C12500 Hard Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C12500 Standards with similar compositions

South Africa: 806 to SABS 806, 807 to SABS 807
UK: C106 to BS 2873
USA: C12500, C12510, C14530, C14530 to ASTM B152M, C14530 to ASTM B888, FRTP to ASTM B216, UNS C12500, UNS C12510, UNS C12700, UNS C12800, UNS C13000, UNS C14530
Tradenames: A-COPPER, PCLW-SNX ALLOY, PMX ALLOY C14530, SELENIUM COPPER-948