C14200 Phosphorus De-Oxidized Arsenical H.C. Copper, Hard Material Data Sheet

C14200 Phosphorus De-Oxidized Arsenical H.C. Copper Material Data Sheet (Wrought, Hard)

C14200 Hard Deoxidized Arsenical Overview

C14200 hard deoxidized arsenical is a wrought general purpose copper (UNS C14200, EN CW117C), known as phosphorus de-oxidized arsenical h.c. copper. Condition: Hard. This C14200 hard deoxidized arsenical material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14200 copper parts in-house and inspects them before shipment.

C14200 Designation

Wrought Copper Alloy: gp-Cu-DPA(h); C107 (UNS C14200)
ConditionHard
UNS numberC14200
EN nameCW117C
ISO nameCuSn0,15

C14200 Typical uses

Heat exchangers, fireboxes, steam pipes, vats, kettles, autoclaves.

C14200 Hard Deoxidized Arsenical Composition detail

As (arsenic)0.15–0.5%
Cu (copper)99.5–99.8%
P (phosphorus)0.013–0.05%

C14200 Physical properties

Density8.92–8.93g/cm3

C14200 Hard Deoxidized Arsenical Mechanical properties

Young’s modulus128–135GPa
Specific stiffness14.3–15.1MN.m/kg
Yield strength (elastic limit)190–340MPa
Tensile strength270–380MPa
Specific strength21.3–38.1kN.m/kg
Elongation6–25% strain
Compressive strength190–340MPa
Flexural modulus128–135GPa
Flexural strength (modulus of rupture)190–340MPa
Shear modulus45–50GPa
Bulk modulus138–146GPa
Poisson’s ratio0.34–0.35 
Shape factor27
Hardness – Vickers83–115HV
Elastic stored energy (springs)147–412kJ/m3
Fatigue strength at 10^7 cycles110–130MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
85.3–168MPa

C14200 Impact & fracture properties

Fracture toughness38.8–55.9MPa.m0.5
Toughness (G)11.8–23.1kJ/m2

C14200 Hard Deoxidized Arsenical Thermal properties

Melting point1050–1080°C
Maximum service temperature120–130°C
Minimum service temperature-273  °C
Thermal conductivity145–186W/m.°C
Specific heat capacity378–383J/kg.°C
Thermal expansion coefficient17–18µstrain/°C
Thermal shock resistance82.5–148°C
Thermal distortion resistance8.27–10.7MW/m
Latent heat of fusion200–208kJ/kg

C14200 Electrical properties

Electrical resistivity3.8–4.9µohm.cm
Electrical conductivity35.2–45.4%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C14200 Magnetic properties

Magnetic typeNon-magnetic

C14200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3790–3890m/s
Mechanical loss coefficient (tan delta)3.5e-5–1.11e-4 

C14200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingAcceptable
Machining speed51.8 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required, and contains hazardous elements
Good

C14200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C14200 Hard Deoxidized Arsenical Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C14200 Notes

C14200 Hard Deoxidized Arsenical Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C14200 Standards with similar compositions

International: CuAs(P) to ISO 1635, CuAs(P) to ISO 1637, CuAs(P) to ISO 1640
Switzerland: Cu-DPA to VSM 11557/1
USA: C14200, C14200 to ASTM B111M, C14200 to ASTM B152M, C14200 to ASTM B359M, C14200 to ASTM B379, C14200 to ASTM B395M, C14200 to ASTM B447, C14200 to ASTM B75M, UNS C14100, UNS C14200, UNS C14210
Tradenames: ARSENICAL COPPER, BRIDGEPORT NO. 108, IMI 146, NORANDA-113, PHOSPHORIZED ARSENICAL COPPER-142, REVERE ALLOY NO. 99, REVERE NO. 142, WOLVERINE ALLOY 02