PEKK Unfilled Semi-Crystalline Material Data Sheet

PEKK Unfilled Semi-Crystalline (Polyetherketoneketone) Material Data Sheet

PEKK Unfilled Semi-Crystalline Overview

PEKK unfilled semi-crystalline is a grade of polyetherketoneketone (PEKK), designated Polyetherketoneketone (unfilled, semi-crystalline). This PEKK unfilled semi-crystalline material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PEKK parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PEKK parts in-house and inspects them before shipment.

PEKK Designation

Polyetherketoneketone (unfilled, semi-crystalline)
TradenamesOxpekk, Pyramid

PEKK Unfilled Semi-Crystalline Composition detail

Polymer100  %

PEKK Physical properties

Density1.3–1.32g/cm3

PEKK Unfilled Semi-Crystalline Mechanical properties

Young’s modulus4.29–4.52GPa
Specific stiffness3.27–3.45MN.m/kg
Yield strength (elastic limit)135–141MPa
Tensile strength105–116MPa
Specific strength103–108kN.m/kg
Elongation11.1–12.9% strain
Elongation at yield5–7% strain
Compressive modulus4.29–4.52GPa
Compressive strength197–217MPa
Flexural modulus4.46–4.69GPa
Flexural strength (modulus of rupture)188–198MPa
Shear modulus1.6–1.7GPa
Shear strength135–141MPa
Poisson’s ratio0.392–0.408 
Shape factor4.2
Hardness – Vickers33–35HV
Hardness – Rockwell M84–92 
Elastic stored energy (springs)2060–2270kJ/m3
Fatigue strength at 10^7 cycles41.8–46.2MPa

PEKK Impact & fracture properties

Impact strength, notched 23 °C4.96–7.28kJ/m2
Impact strength, unnotched 23 °C40–58kJ/m2

PEKK Unfilled Semi-Crystalline Thermal properties

Melting point347–373°C
Glass temperature153–170°C
Heat deflection temperature 0.45MPa170–188°C
Heat deflection temperature 1.8MPa166–184°C
Vicat softening point170–188°C
Thermal conductivity0.25  W/m.°C
Specific heat capacity1510–1540J/kg.°C
Thermal expansion coefficient21–38µstrain/°C
Thermal shock resistance823–1490°C
Thermal distortion resistance0.00658–0.0119MW/m

PEKK Electrical properties

Electrical resistivity10000000000000000  µohm.cm
Electrical conductivity1.72e-14 %IACS
Dielectric constant (relative permittivity)3.17–3.43 
Dissipation factor (dielectric loss tangent)0.0035–0.0045 
Dielectric strength (dielectric breakdown)23–25MV/m

PEKK Magnetic properties

Magnetic typeNon-magnetic

PEKK Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1810–1860m/s

PEKK Absorption & permeability

Water absorption @ 24 hrs0.27–0.33%

PEKK Processing properties

Polymer injection moldingAcceptable
Polymer extrusionLimited use
Polymer thermoformingUnsuitable
Linear mold shrinkage1.3 – 1.5 %

PEKK Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oils and fuelsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Excellent
FlammabilitySelf-extinguishing