PPA General Purpose Grade (Polyphthalamide) Material Data Sheet
PPA General Purpose Grade Overview
PPA general purpose grade is a grade of polyphthalamide (PPA), designated Polyphthalamide (Unreinforced). This PPA general purpose grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.
PPA General Purpose Grade Designation
Polyphthalamide (Unreinforced) Tradenames Akromid, Amodel, Arlen, Badamid, Durethan, Lubriloy, Novamid, Sepaz, Star-Therm, Tecomid, Terez, Tribocomp, Vampamid, Vestamid Htplus, Zytel
PPA General Purpose Grade Typical uses
Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications
PPA General Purpose Grade Composition detail
PPA General Purpose Grade Physical properties
PPA General Purpose Grade Mechanical properties
Young’s modulus 1.64 – 2.04 GPa Specific stiffness 1.44 – 1.79 MN.m/kg Yield strength (elastic limit) 44.3 – 55.2 MPa Tensile strength 63 – 77.1 MPa Specific strength 38.8 – 48.4 kN.m/kg Elongation 24.6 – 35.4 % strain Elongation at yield 8.63 – 16.4 % strain Compressive modulus 1.75 – 1.93 GPa Compressive strength 79.9 – 88.3 MPa Flexural modulus 3 – 3.6 GPa Flexural strength (modulus of rupture) 85.7 – 105 MPa Shear modulus 0.641 – 0.674 GPa Shear strength 37.8 – 46.2 MPa Bulk modulus 2.85 – 3.15 GPa Poisson’s ratio 0.383 – 0.398 Shape factor 4.5 Hardness – Vickers 14 – 16 HV Hardness – Rockwell M 121 – 133 Hardness – Rockwell R 121 – 133 Hardness – Shore D 83 – 86 Elastic stored energy (springs) 531 – 842 kJ/m3 Fatigue strength at 10^7 cycles 26.6 – 29.4 MPa
PPA General Purpose Grade Impact & fracture properties
Fracture toughness 3.46 – 3.82 MPa.m0.5 Toughness (G) 6.26 – 8.34 kJ/m2 Impact strength, notched 23 °C 13.8 – 26.8 kJ/m2 Impact strength, notched -30 °C 6.99 – 15.2 kJ/m2 Impact strength, unnotched 23 °C 590 – 600 kJ/m2 Impact strength, unnotched -30 °C 590 – 600 kJ/m2
PPA General Purpose Grade Thermal properties
Melting point 299 – 322 °C Glass temperature 119 – 135 °C Heat deflection temperature 0.45MPa 126 – 166 °C Heat deflection temperature 1.8MPa 101 – 140 °C Maximum service temperature 108 – 124 °C Minimum service temperature -49 – -29 °C Thermal conductivity 0.2 – 0.25 W/m.°C Specific heat capacity 1560 – 1620 J/kg.°C Thermal expansion coefficient 90 – 95 µstrain/°C Thermal shock resistance 251 – 341 °C Thermal distortion resistance 0.00216 – 0.00271 MW/m
PPA General Purpose Grade Electrical properties
Electrical resistivity 1.64e20 – 4.1e21 µohm.cm Electrical conductivity 4.21e-20 – 1.05e-18 %IACS Dielectric constant (relative permittivity) 2.99 – 4.21 Dissipation factor (dielectric loss tangent) 0.0066 – 0.0174 Dielectric strength (dielectric breakdown) 12.6 – 21.4 MV/m Comparative tracking index 600 V
PPA General Purpose Grade Magnetic properties
Magnetic type Non-magnetic
PPA General Purpose Grade Optical, aesthetic and acoustic properties
Transparency Translucent Acoustic velocity 1200 – 1340 m/s Mechanical loss coefficient (tan delta) 0.0138 – 0.0153
PPA General Purpose Grade Absorption & permeability
Water absorption @ 24 hrs 0.68 – 1.1 % Water absorption @ sat 8.3 – 11 % Humidity absorption @ sat 2.3 – 3.1 %
PPA General Purpose Grade Processing properties
Polymer injection molding Excellent Polymer extrusion Unsuitable Polymer thermoforming Limited use Linear mold shrinkage 1.5 – 2 % Melt temperature 268 – 349 °C Molding pressure range 34.4 – 103 MPa
PPA General Purpose Grade Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Excellent Strong acids Limited use Weak alkalis Excellent Strong alkalis Limited use Organic solvents Limited use Oxidation at 500C Unacceptable UV radiation (sunlight) Fair Flammability Slow-burning