PPA Extra Tough Grade Material Data Sheet

PPA Extra Tough Grade (Polyphthalamide) Material Data Sheet

PPA Extra Tough Grade Overview

PPA extra tough grade is a grade of polyphthalamide (PPA), designated Polyphthalamide (Extra tough). This PPA extra tough grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.

PPA Extra Tough Grade Designation

Polyphthalamide (Extra tough)
TradenamesAmodel, Tecomid, Zytel

PPA Extra Tough Grade Typical uses

Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications

PPA Extra Tough Grade Composition detail

Polymer75–85%
Impact modifier15–25%

PPA Extra Tough Grade Physical properties

Density1.1–1.12g/cm3

PPA Extra Tough Grade Mechanical properties

Young’s modulus2.05–2.55GPa
Specific stiffness1.85–2.3MN.m/kg
Yield strength (elastic limit)56.4–70.3MPa
Tensile strength68.4–83.6MPa
Specific strength50.8–63.4kN.m/kg
Elongation24.6–35.4% strain
Elongation at yield8.63–16.4% strain
Compressive modulus2.19–2.42GPa
Compressive strength86.6–95.8MPa
Flexural modulus2.09–2.51GPa
Flexural strength (modulus of rupture)65.7–80.3MPa
Shear modulus0.796–0.837GPa
Shear strength51.3–62.7MPa
Bulk modulus3.96–4.38GPa
Poisson’s ratio0.392–0.408 
Shape factor4.5
Hardness – Vickers18–20HV
Hardness – Rockwell M126–139 
Hardness – Rockwell R126–139 
Hardness – Shore D84–88 
Elastic stored energy (springs)688–1090kJ/m3
Fatigue strength at 10^7 cycles28.9–31.9MPa

PPA Extra Tough Grade Impact & fracture properties

Fracture toughness3.62–4MPa.m0.5
Toughness (G)5.49–7.31kJ/m2
Impact strength, notched 23 °C66–128kJ/m2
Impact strength, notched -30 °C15.8–34.3kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PPA Extra Tough Grade Thermal properties

Melting point299–322°C
Glass temperature119–135°C
Heat deflection temperature 0.45MPa126–166°C
Heat deflection temperature 1.8MPa101–140°C
Maximum service temperature108–124°C
Minimum service temperature-49–-29°C
Thermal conductivity0.255–0.265W/m.°C
Specific heat capacity1600–1660J/kg.°C
Thermal expansion coefficient58.3–60.7µstrain/°C
Thermal shock resistance397–539°C
Thermal distortion resistance0.00425–0.0045MW/m

PPA Extra Tough Grade Electrical properties

Electrical resistivity2e21–5e22µohm.cm
Electrical conductivity3.45e-21–8.62e-20%IACS
Dielectric constant (relative permittivity)2.99–4.21 
Dissipation factor (dielectric loss tangent)0.0066–0.0174 
Dielectric strength (dielectric breakdown)12.6–21.4MV/m
Comparative tracking index600  V

PPA Extra Tough Grade Magnetic properties

Magnetic typeNon-magnetic

PPA Extra Tough Grade Optical, aesthetic and acoustic properties

TransparencyTranslucent
Acoustic velocity1360–1520m/s
Mechanical loss coefficient (tan delta)0.0166–0.0183 

PPA Extra Tough Grade Absorption & permeability

Water absorption @ 24 hrs0.38–0.62%
Water absorption @ sat5.4–7.2%
Humidity absorption @ sat1.6–2.2%

PPA Extra Tough Grade Processing properties

Polymer injection moldingExcellent
Polymer extrusionUnsuitable
Polymer thermoformingLimited use
Linear mold shrinkage1.5 – 2 %
Melt temperature268 – 349 °C
Molding pressure range34.4 – 103 MPa

PPA Extra Tough Grade Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsLimited use
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsLimited use
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning