PPA 51% Glass and Mineral (Polyphthalamide) Material Data Sheet
PPA 51% Glass and Mineral Overview
PPA 51% glass and mineral is a grade of polyphthalamide (PPA), designated Polyphthalamide (51% glass and mineral). This PPA 51% glass and mineral material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.
PPA 51% Glass and Mineral Designation
Polyphthalamide (51% glass and mineral)
Tradenames
Zytel
PPA 51% Glass and Mineral Typical uses
Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications
PPA 51% Glass and Mineral Composition detail
Polymer
49
%
Glass (fiber)
15
–
36
%
Mineral (unspecified)
15
–
36
%
PPA 51% Glass and Mineral Physical properties
Density
1.65
–
1.68
g/cm3
PPA 51% Glass and Mineral Mechanical properties
Young’s modulus
13.4
–
16.7
GPa
Specific stiffness
8.05
–
10
MN.m/kg
Yield strength (elastic limit)
156
–
194
MPa
Tensile strength
158
–
193
MPa
Specific strength
93.7
–
117
kN.m/kg
Elongation
1.63
–
2.35
% strain
Elongation at yield
1.38
–
2.61
% strain
Compressive modulus
14.3
–
15.8
GPa
Compressive strength
200
–
221
MPa
Flexural modulus
11.6
–
13.9
GPa
Flexural strength (modulus of rupture)
242
–
296
MPa
Shear modulus
5.39
–
5.67
GPa
Shear strength
94.5
–
116
MPa
Bulk modulus
16.9
–
18.7
GPa
Poisson’s ratio
0.345
–
0.359
Shape factor
7.39
Hardness – Vickers
50
–
55
HV
Hardness – Rockwell M
184
–
204
Hardness – Rockwell R
184
–
204
Hardness – Shore D
98
–
102
Elastic stored energy (springs)
804
–
1270
kJ/m3
Fatigue strength at 10^7 cycles
66.5
–
73.5
MPa
PPA 51% Glass and Mineral Impact & fracture properties
Fracture toughness
5.29
–
5.85
MPa.m0.5
Toughness (G)
1.79
–
2.39
kJ/m2
Impact strength, notched 23 °C
8.45
–
16.4
kJ/m2
Impact strength, notched -30 °C
7.25
–
15.8
kJ/m2
Impact strength, unnotched 23 °C
67.5
–
99.2
kJ/m2
Impact strength, unnotched -30 °C
64.7
–
97
kJ/m2
PPA 51% Glass and Mineral Thermal properties
Melting point
299
–
322
°C
Glass temperature
119
–
135
°C
Heat deflection temperature 0.45MPa
250
–
303
°C
Heat deflection temperature 1.8MPa
225
–
276
°C
Maximum service temperature
195
–
214
°C
Minimum service temperature
-49
–
-29
°C
Thermal conductivity
0.511
–
0.531
W/m.°C
Specific heat capacity
1210
–
1260
J/kg.°C
Thermal expansion coefficient
20
–
43
µstrain/°C
Thermal shock resistance
265
–
593
°C
Thermal distortion resistance
0.0121
–
0.0261
MW/m
PPA 51% Glass and Mineral Electrical properties
Electrical resistivity
1.37e18
–
3.42e19
µohm.cm
Electrical conductivity
5.04e-18
–
1.26e-16
%IACS
Dielectric constant (relative permittivity)
4.15
–
5.85
Dissipation factor (dielectric loss tangent)
0.145
–
0.381
Dielectric strength (dielectric breakdown)
24.7
–
42.1
MV/m
Comparative tracking index
600
V
PPA 51% Glass and Mineral Magnetic properties
Magnetic type
Non-magnetic
PPA 51% Glass and Mineral Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2830
–
3170
m/s
Mechanical loss coefficient (tan delta)
0.00704
–
0.00778
PPA 51% Glass and Mineral Absorption & permeability