PPA 40% Glass and Mineral (Polyphthalamide) Material Data Sheet
PPA 40% Glass and Mineral Overview
PPA 40% glass and mineral is a grade of polyphthalamide (PPA), designated Polyphthalamide (40% glass and mineral). This PPA 40% glass and mineral material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.
PPA 40% Glass and Mineral Designation
Polyphthalamide (40% glass and mineral)
Tradenames
Zytel
PPA 40% Glass and Mineral Typical uses
Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications
PPA 40% Glass and Mineral Composition detail
Polymer
60
%
Glass (fiber)
10
–
30
%
Mineral (unspecified)
10
–
30
%
PPA 40% Glass and Mineral Physical properties
Density
1.49
–
1.52
g/cm3
PPA 40% Glass and Mineral Mechanical properties
Young’s modulus
9.49
–
11.8
GPa
Specific stiffness
6.3
–
7.84
MN.m/kg
Yield strength (elastic limit)
127
–
158
MPa
Tensile strength
128
–
157
MPa
Specific strength
84.4
–
105
kN.m/kg
Elongation
1.77
–
2.54
% strain
Elongation at yield
1.49
–
2.82
% strain
Compressive modulus
10.1
–
11.2
GPa
Compressive strength
162
–
180
MPa
Flexural modulus
8.55
–
10.2
GPa
Flexural strength (modulus of rupture)
216
–
263
MPa
Shear modulus
3.8
–
3.99
GPa
Shear strength
77
–
94.1
MPa
Bulk modulus
12.8
–
14.1
GPa
Poisson’s ratio
0.354
–
0.368
Shape factor
6.7
Hardness – Vickers
41
–
45
HV
Hardness – Rockwell M
172
–
190
Hardness – Rockwell R
172
–
190
Hardness – Shore D
95
–
99
Elastic stored energy (springs)
754
–
1190
kJ/m3
Fatigue strength at 10^7 cycles
54.2
–
59.9
MPa
PPA 40% Glass and Mineral Impact & fracture properties
Fracture toughness
4.93
–
5.45
MPa.m0.5
Toughness (G)
2.2
–
2.93
kJ/m2
Impact strength, notched 23 °C
2.72
–
5.28
kJ/m2
Impact strength, notched -30 °C
1.89
–
4.11
kJ/m2
Impact strength, unnotched 23 °C
34
–
50
kJ/m2
Impact strength, unnotched -30 °C
24
–
36
kJ/m2
PPA 40% Glass and Mineral Thermal properties
Melting point
300
–
322
°C
Glass temperature
119
–
135
°C
Heat deflection temperature 0.45MPa
274
–
329
°C
Heat deflection temperature 1.8MPa
249
–
302
°C
Maximum service temperature
210
–
229
°C
Minimum service temperature
-49
–
-29
°C
Thermal conductivity
0.448
–
0.466
W/m.°C
Specific heat capacity
1290
–
1340
J/kg.°C
Thermal expansion coefficient
26
–
48
µstrain/°C
Thermal shock resistance
272
–
528
°C
Thermal distortion resistance
0.00951
–
0.0176
MW/m
PPA 40% Glass and Mineral Electrical properties
Electrical resistivity
1.5e20
–
3.76e21
µohm.cm
Electrical conductivity
4.59e-20
–
1.15e-18
%IACS
Dielectric constant (relative permittivity)
3.27
–
4.61
Dissipation factor (dielectric loss tangent)
0.00385
–
0.0102
Dielectric strength (dielectric breakdown)
18.7
–
31.9
MV/m
Comparative tracking index
550
–
600
V
PPA 40% Glass and Mineral Magnetic properties
Magnetic type
Non-magnetic
PPA 40% Glass and Mineral Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2510
–
2800
m/s
Mechanical loss coefficient (tan delta)
0.0082
–
0.00906
PPA 40% Glass and Mineral Absorption & permeability