PA612 Toughened Grade Material Data Sheet

PA612 Toughened Grade (Polyamide 612) Material Data Sheet

PA612 Toughened Grade Overview

PA612 toughened grade is a grade of polyamide 612 (PA612, nylon 612), designated Polyamide (Nylon) (Type 612, Unreinforced, Toughened). This PA612 toughened grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA612 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA612 parts in-house and inspects them before shipment.

PA612 Toughened Grade Designation

Polyamide (Nylon) (Type 612, Unreinforced, Toughened)
TradenamesSchulamid, Vestamid

PA612 Toughened Grade Typical uses

Mechanical parts, zips, filaments, coverings and coatings requiring abrasion resistance.

PA612 Toughened Grade Composition detail

Polymer85–97%
Impact modifier3–15%

PA612 Toughened Grade Physical properties

Density1–1.02g/cm3

PA612 Toughened Grade Mechanical properties

Young’s modulus0.49–0.611GPa
Specific stiffness0.485–0.605MN.m/kg
Yield strength (elastic limit)19.6–24.4MPa
Tensile strength24.8–30.3MPa
Specific strength19.4–24.2kN.m/kg
Elongation55.4–79.7% strain
Elongation at yield24.2–45.9% strain
Compressive modulus0.523–0.578GPa
Compressive strength31.4–34.7MPa
Flexural modulus0.735–0.88GPa
Flexural strength (modulus of rupture)24.8–30.3MPa
Shear modulus0.189–0.198GPa
Shear strength14.9–18.2MPa
Bulk modulus1.12–1.23GPa
Poisson’s ratio0.405–0.422 
Shape factor3.8
Hardness – Vickers6–7HV
Hardness – Rockwell M69–76 
Hardness – Rockwell R69–76 
Hardness – Shore D66–69 
Elastic stored energy (springs)347–550kJ/m3
Fatigue strength at 10^7 cycles10.5–11.6MPa

PA612 Toughened Grade Impact & fracture properties

Fracture toughness2.71–3MPa.m0.5
Toughness (G)12.8–17.2kJ/m2
Impact strength, notched 23 °C54.4–106kJ/m2
Impact strength, notched -30 °C8.19–17.8kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA612 Toughened Grade Thermal properties

Melting point195–217°C
Glass temperature40–52°C
Heat deflection temperature 0.45MPa66–100°C
Heat deflection temperature 1.8MPa41–74°C
Maximum service temperature42–57°C
Minimum service temperature-127–-107°C
Thermal conductivity0.213–0.222W/m.°C
Specific heat capacity1710–1780J/kg.°C
Thermal expansion coefficient167–170µstrain/°C
Thermal shock resistance204–277°C
Thermal distortion resistance0.00127–0.00132MW/m

PA612 Toughened Grade Electrical properties

Electrical resistivity2.46e21–6.15e22µohm.cm
Electrical conductivity2.8e-21–7.01e-20%IACS
Dielectric constant (relative permittivity)4.26–6.01 
Dissipation factor (dielectric loss tangent)0.0431–0.114 
Dielectric strength (dielectric breakdown)23.5–40.1MV/m
Comparative tracking index600  V

PA612 Toughened Grade Magnetic properties

Magnetic typeNon-magnetic

PA612 Toughened Grade Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity695–779m/s
Mechanical loss coefficient (tan delta)0.028–0.0309 

PA612 Toughened Grade Absorption & permeability

Water absorption @ 24 hrs0.54–0.88%
Water absorption @ sat2.4–3.1%
Humidity absorption @ sat1–1.4%
Permeability (O2)36.5–86cm³.mm/m².day.atm

PA612 Toughened Grade Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage1 – 1.21 %
Melt temperature213 – 288 °C
Mold temperature30 – 60 °C
Molding pressure range6.88 – 103 MPa

PA612 Toughened Grade Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning