PA612 10% PTFE Lubricated Material Data Sheet

PA612 10% PTFE Lubricated (Polyamide 612) Material Data Sheet

PA612 10% PTFE Lubricated Overview

PA612 10% PTFE lubricated is a grade of polyamide 612 (PA612, nylon 612), designated Polyamide (Nylon) (Type 612, 10% PTFE, Lubricated). This PA612 10% PTFE lubricated material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA612 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA612 parts in-house and inspects them before shipment.

PA612 10% PTFE Lubricated Designation

Polyamide (Nylon) (Type 612, 10% PTFE, Lubricated)
TradenamesLNP Lubricomp, Lubrione, Nycal, Plaslube, Radici, Zytel

PA612 10% PTFE Lubricated Typical uses

Mechanical parts, zips, filaments, coverings and coatings requiring abrasion resistance.

PA612 10% PTFE Lubricated Composition detail

Polymer90  %
PTFE (lubricant)10  %

PA612 10% PTFE Lubricated Physical properties

Density1.1–1.13g/cm3

PA612 10% PTFE Lubricated Mechanical properties

Young’s modulus1.49–1.86GPa
Specific stiffness1.34–1.67MN.m/kg
Yield strength (elastic limit)43.6–54.4MPa
Tensile strength52.9–64.7MPa
Specific strength39.1–48.8kN.m/kg
Elongation55.4–79.7% strain
Elongation at yield24.2–45.9% strain
Compressive modulus1.59–1.76GPa
Compressive strength67–74.1MPa
Flexural modulus1.58–1.89GPa
Flexural strength (modulus of rupture)70.1–85.6MPa
Shear modulus0.569–0.598GPa
Shear strength31.7–38.8MPa
Bulk modulus4.14–4.58GPa
Poisson’s ratio0.42–0.436 
Shape factor4.4
Hardness – Vickers14–15HV
Hardness – Rockwell M110–121 
Hardness – Rockwell R110–121 
Hardness – Shore D80–83 
Elastic stored energy (springs)565–899kJ/m3
Fatigue strength at 10^7 cycles22.3–24.7MPa

PA612 10% PTFE Lubricated Impact & fracture properties

Fracture toughness3.4–3.75MPa.m0.5
Toughness (G)6.63–8.84kJ/m2
Impact strength, notched 23 °C5.01–9.72kJ/m2
Impact strength, notched -30 °C3.33–7.24kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA612 10% PTFE Lubricated Thermal properties

Melting point195–217°C
Glass temperature40–52°C
Heat deflection temperature 0.45MPa102–140°C
Heat deflection temperature 1.8MPa77–113°C
Maximum service temperature90–120°C
Minimum service temperature-127–-107°C
Thermal conductivity0.185–0.192W/m.°C
Specific heat capacity1600–1660J/kg.°C
Thermal expansion coefficient99–101µstrain/°C
Thermal shock resistance251–341°C
Thermal distortion resistance0.00184–0.00192MW/m

PA612 10% PTFE Lubricated Electrical properties

Electrical resistivity2.46e21–6.15e22µohm.cm
Electrical conductivity2.8e-21–7.01e-20%IACS
Dielectric constant (relative permittivity)4.26–6.01 
Dissipation factor (dielectric loss tangent)0.0428–0.113 
Dielectric strength (dielectric breakdown)23.5–40.1MV/m
Comparative tracking index600  V

PA612 10% PTFE Lubricated Magnetic properties

Magnetic typeNon-magnetic

PA612 10% PTFE Lubricated Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1150–1290m/s
Mechanical loss coefficient (tan delta)0.0191–0.0211 

PA612 10% PTFE Lubricated Absorption & permeability

Water absorption @ 24 hrs0.48–0.79%
Water absorption @ sat2.1–2.8%
Humidity absorption @ sat0.9–1.2%

PA612 10% PTFE Lubricated Processing properties

Polymer injection moldingExcellent
Polymer extrusionUnsuitable
Polymer thermoformingLimited use
Linear mold shrinkage1.09 – 1.32 %
Melt temperature213 – 288 °C
Mold temperature30 – 60 °C
Molding pressure range27.5 – 138 MPa

PA612 10% PTFE Lubricated Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning