PA12 Rigid Grade Material Data Sheet

PA12 Rigid Grade (Polyamide 12) Material Data Sheet

PA12 Rigid Grade Overview

PA12 rigid grade is a grade of polyamide 12 (PA12, nylon 12), designated Polyamide (Nylon) (Type 12, Molding and Extrusion). This PA12 rigid grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA12 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA12 parts in-house and inspects them before shipment.

PA12 Rigid Grade Designation

Polyamide (Nylon) (Type 12, Molding and Extrusion)
TradenamesAshlene, Badamid, Dynastat, Fostalon, Fostamid, Gravi-Tech, Grilamid, Hifill, Latimass, Luvocom, Pentamid, Plustek, Rilsamid, Rilsan, Schulamid, Therma-Tech, Ubesta, Vestamid, Vestosint

PA12 Rigid Grade Typical uses

Precision engineering components, components requiring low temperature toughness, sports shoe soles.

PA12 Rigid Grade Composition detail

Polymer100  %

PA12 Rigid Grade Physical properties

Density1–1.02g/cm3

PA12 Rigid Grade Mechanical properties

Young’s modulus1.08–1.35GPa
Specific stiffness1.07–1.34MN.m/kg
Yield strength (elastic limit)34.8–43.4MPa
Tensile strength45–55MPa
Specific strength34.4–43kN.m/kg
Elongation41–59% strain
Elongation at yield7.03–13.3% strain
Compressive modulus1.08–1.35GPa
Compressive strength57–63MPa
Flexural modulus1.17–1.2GPa
Flexural strength (modulus of rupture)57.4–70.1MPa
Shear modulus0.418–0.439GPa
Shear strength27–33MPa
Bulk modulus2.47–2.74GPa
Poisson’s ratio0.406–0.422 
Shape factor4.19
Hardness – Vickers11–12HV
Hardness – Rockwell M70–80 
Hardness – Rockwell R100–110 
Hardness – Brinell62–78HB
Hardness – Shore D69–71 
Elastic stored energy (springs)496–789kJ/m3
Fatigue strength at 10^7 cycles19–21MPa

PA12 Rigid Grade Impact & fracture properties

Fracture toughness3.18–3.52MPa.m0.5
Toughness (G)8.01–10.7kJ/m2
Impact strength, notched 23 °C15.1–29.3kJ/m2
Impact strength, notched -30 °C5.04–11kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA12 Rigid Grade Thermal properties

Melting point170–178°C
Glass temperature40–43°C
Heat deflection temperature 0.45MPa70–94°C
Heat deflection temperature 1.8MPa35–57°C
Maximum service temperature80–110°C
Minimum service temperature-67–-47°C
Thermal conductivity0.218–0.306W/m.°C
Specific heat capacity1680–1720J/kg.°C
Thermal expansion coefficient110–180µstrain/°C
Thermal shock resistance173–304°C
Thermal distortion resistance0.00138–0.00245MW/m

PA12 Rigid Grade Electrical properties

Electrical resistivity2.81e19–7.03e20µohm.cm
Electrical conductivity2.45e-19–6.14e-18%IACS
Dielectric constant (relative permittivity)4.2–5.92 
Dissipation factor (dielectric loss tangent)0.0473–0.125 
Dielectric strength (dielectric breakdown)23.4–39.8MV/m
Comparative tracking index600  V

PA12 Rigid Grade Magnetic properties

Magnetic typeNon-magnetic

PA12 Rigid Grade Optical, aesthetic and acoustic properties

Refractive index1.52–1.54 
TransparencyTranslucent
Acoustic velocity1030–1160m/s
Mechanical loss coefficient (tan delta)0.02–0.07 

PA12 Rigid Grade Absorption & permeability

Water absorption @ 24 hrs0.53–0.87%
Water absorption @ sat1.4–1.8%
Humidity absorption @ sat0.62–0.84%
Water vapor transmission0.35  g.mm/m².day
Permeability (O2)35  cm³.mm/m².day.atm

PA12 Rigid Grade Processing properties

Polymer injection moldingExcellent
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.8 – 1.5 %
Melt temperature177 – 274 °C
Mold temperature40 – 60 °C
Molding pressure range16 – 75 MPa

PA12 Rigid Grade Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsAcceptable
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilityHighly flammable