PA12 Flexible Grade Material Data Sheet

PA12 Flexible Grade (Polyamide 12) Material Data Sheet

PA12 Flexible Grade Overview

PA12 flexible grade is a grade of polyamide 12 (PA12, nylon 12), designated Polyamide (Nylon) (Type 12, flexible, molding and extrusion). This PA12 flexible grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA12 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA12 parts in-house and inspects them before shipment.

PA12 Flexible Grade Designation

Polyamide (Nylon) (Type 12, flexible, molding and extrusion)
TradenamesAshlene, Grilamid, Rilsan, Ubesta, Vestamid

PA12 Flexible Grade Typical uses

Precision engineering components, components requiring low temperature toughness, sports shoe soles, pipes and tubes for automotive fuel and brake lines.

PA12 Flexible Grade Composition detail

Polymer87–93%
Plasticizer/oil7–13%

PA12 Flexible Grade Physical properties

Density1.03–1.04g/cm3

PA12 Flexible Grade Mechanical properties

Young’s modulus0.35–0.42GPa
Specific stiffness0.338–0.406MN.m/kg
Yield strength (elastic limit)22–25MPa
Tensile strength40  MPa
Specific strength21.3–24.2kN.m/kg
Elongation360  % strain
Elongation at yield20–26% strain
Compressive modulus0.35–0.42GPa
Compressive strength48  MPa
Flexural modulus0.35–0.42GPa
Flexural strength (modulus of rupture)31.9–36.3MPa
Shear modulus0.13–0.15GPa
Shear strength24  MPa
Bulk modulus0.621–0.897GPa
Poisson’s ratio0.406–0.422 
Shape factor3.3
Hardness – Vickers9–10HV
Hardness – Rockwell M45
Hardness – Rockwell R75
Hardness – Shore D63–65 
Elastic stored energy (springs)617–834kJ/m3
Fatigue strength at 10^7 cycles16  MPa

PA12 Flexible Grade Impact & fracture properties

Fracture toughness2.6–2.7MPa.m0.5
Toughness (G)16.7–20.2kJ/m2
Impact strength, notched 23 °C25–30kJ/m2
Impact strength, notched -30 °C4–13kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA12 Flexible Grade Thermal properties

Melting point171–174°C
Glass temperature40–43°C
Heat deflection temperature 0.45MPa90–95°C
Heat deflection temperature 1.8MPa45–46°C
Vicat softening point125–130°C
Maximum service temperature80–110°C
Minimum service temperature-67–-47°C
Thermal conductivity0.218–0.306W/m.°C
Specific heat capacity1680–1720J/kg.°C
Thermal expansion coefficient140–180µstrain/°C
Thermal shock resistance327–454°C
Thermal distortion resistance0.00132–0.002MW/m
Latent heat of fusion65–75kJ/kg

PA12 Flexible Grade Electrical properties

Electrical resistivity1e17–1e19µohm.cm
Electrical conductivity1.72e-17–1.72e-15%IACS
Dielectric constant (relative permittivity)4.2–16 
Dissipation factor (dielectric loss tangent)0.15–0.2 
Dielectric strength (dielectric breakdown)24–32MV/m
Comparative tracking index600  V

PA12 Flexible Grade Magnetic properties

Magnetic typeNon-magnetic

PA12 Flexible Grade Optical, aesthetic and acoustic properties

Refractive index1.52–1.54 
TransparencyTranslucent
Acoustic velocity581–638m/s
Mechanical loss coefficient (tan delta)0.09–0.12 

PA12 Flexible Grade Absorption & permeability

Water absorption @ 24 hrs0.2  %
Water absorption @ sat1.2–1.4%
Humidity absorption @ sat0.5–0.7%
Water vapor transmission0.28  g.mm/m².day
Permeability (O2)30  cm³.mm/m².day.atm

PA12 Flexible Grade Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.9 – 1.3 %
Melt temperature230 – 270 °C
Mold temperature40 – 80 °C
Molding pressure range16 – 75 MPa

PA12 Flexible Grade Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsAcceptable
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilityHighly flammable