INCONEL X-750, equalized & aged, Nickel-chromium alloy, Material Data Sheet

Nickel-chromium alloy, INCONEL X-750, equalized & aged

INCONEL X-750, equalized & aged, Designation

Wrought Ni-Cr alloy: Inconel X-750, Equalized and Aged
ConditionEqualized & aged
UNS numberN07750
US nameASTM Grade N07750 Type 1; AMS 5542, 5598, 5667-5671, 5747, 5698,5699
EN nameNiCr15Fe7TiAl
EN number2.4669
ISO nameISO 9723-9725, 6208

INCONEL X-750, equalized & aged, Tradenames

INCONEL X-750Special Metals Corp. (USA)
HPM X750Hamilton Precision Metals (USA)
ALTEMP X750ATI Allegheny Ludlum (USA)
NICKELVAC X750ATI Allvac (USA)

INCONEL X-750, equalized & aged, Typical uses

Aircraft turbine parts, industrial turbine parts

INCONEL X-750, equalized & aged, Composition detail

Al (aluminum)0.4–1%
C (carbon)0–0.08%
Co (cobalt)0–1%
Cr (chromium)14–17%
Cu (copper)0–0.5%
Fe (iron)5–9%
Mn (manganese)0–1%
Nb (niobium)0.35–0.6%
Ni (nickel)70–75%
S (sulfur)0–0.01%
Si (silicon)0–0.5%
Ta (tantalum)0.35–0.6%
Ti (titanium)2.25–2.75%

INCONEL X-750, equalized & aged, Physical properties

Density 8.21–8.29g/cm3

INCONEL X-750, equalized & aged, Mechanical properties

Young’s modulus211–222GPa
Specific stiffness25.6–26.9MN.m/kg
Yield strength (elastic limit)690–763MPa
Tensile strength1100–1220MPa
Specific strength83.6–92.5kN.m/kg
Elongation15–20% strain
Compressive strength690–763MPa
Flexural modulus211–222GPa
Flexural strength (modulus of rupture)690–763MPa
Shear modulus81–85.2GPa
Bulk modulus176–185GPa
Poisson’s ratio0.3–0.312 
Shape factor22   
Hardness – Vickers320–400HV
Hardness – Rockwell B107–112HRB
Hardness – Rockwell C32–41HRC
Hardness – Brinell303–379HB
Elastic stored energy (springs)1100–1340kJ/m3
Fatigue strength at 10^7 cycles430–660MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
422–672MPa

INCONEL X-750, equalized & aged, Impact & fracture properties

Fracture toughness105–116MPa.m0.5
Toughness (G)50.6–62.4kJ/m2

INCONEL X-750, equalized & aged, Thermal properties

Melting point1390–1430°C
Maximum service temperature732–816°C
Minimum service temperature-273  °C
Thermal conductivity11.4–12.4W/m.°C
Specific heat capacity461–480J/kg.°C
Thermal expansion coefficient13.3–14µstrain/°C
Thermal shock resistance231–261°C
Thermal distortion resistance0.829–0.911MW/m
Latent heat of fusion275–300kJ/kg

INCONEL X-750, equalized & aged, Electrical properties

Electrical resistivity116–127µohm.cm
Electrical conductivity1.36–1.49%IACS
Galvanic potential-0.1–-0.02V

INCONEL X-750, equalized & aged, Magnetic properties

Magnetic typeNon-magnetic

INCONEL X-750, equalized & aged, Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5190m/s
Mechanical loss coefficient (tan delta)2e-4–4e-4 

INCONEL X-750, equalized & aged, Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingLimited use
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed3.96 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good

INCONEL X-750, equalized & aged, Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsExcellent
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Bronze or zinc alloy dies should be used to minimize galling.
Limited use
FlammabilityNon-flammable

INCONEL X-750, equalized & aged, Corrosion resistance of metals

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydroxide
Not susceptible

INCONEL X-750, equalized & aged, Notes

Warning
All nickel compounds should be regarded as toxic.  Some can cause cancer and/or fetal abnormalities.
Other notes
INCONEL is a registered trademark of the INCO group of companies.
As of September 1999 , INCONEL, INCOLOY, MONEL, NIMONIC, INCO-WELD, NILO, BRIGHTRAY, CORRONEL and UDIMET have become registered trademarks of Special Metals Corporation

INCONEL X-750, equalized & aged, Standards with similar compositions

International: NiCr15Fe7Ti2Al to ISO 6208, NiCr15Fe7Ti2Al to ISO 9724, NiCr15Fe7Ti2Al to ISO 9725, NW7750 to ISO 6208, NW7750 to ISO 9724, NW7750 to ISO 9725
USA: N07750 Type 1 to ASTM B637, N07750 Type 2 to ASTM B637, N07750 Type 3 to ASTM B637
Tradenames: INCONEL ALLOY 722, INCONEL ALLOY X-750, P.E.R 20 N