AISI 4135 Normalized Mechanical Properties , Low alloy steel (4100 Series, Cr-Mo Alloyed, 0.35% C )
| AISI 4135 |
| Condition | Normalized |
| Young’s modulus | 200 | – | 210 | GPa |
| Specific stiffness | 25.5 | – | 26.9 | MN.m/kg |
| Yield strength (elastic limit) | 483 | – | 586 | MPa |
| Tensile strength | 621 | – | 690 | MPa |
| Specific strength | 61.7 | – | 74.8 | kN.m/kg |
| Elongation | 8 | – | 18 | % strain |
| Compressive strength | 483 | – | 614 | MPa |
| Flexural modulus | 200 | – | 210 | GPa |
| Flexural strength (modulus of rupture) | 483 | – | 586 | MPa |
| Shear modulus | 76 | – | 79.9 | GPa |
| Bulk modulus | 185 | – | 195 | GPa |
| Poisson’s ratio | 0.32 | – | 0.333 | |
| Shape factor | 45 | | | |
| Hardness – Vickers | 200 | – | 240 | HV |
| Hardness – Brinell | 190 | – | 230 | HB |
| Elastic stored energy (springs) | 573 | – | 831 | kJ/m^3 |
| Fatigue strength at 10^7 cycles | 338 | – | 368 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 311 | – | 400 | MPa |
| AISI 4135 Low alloy steel (4100 Series, Cr-Mo Alloyed, 0.35% C ) | |
|---|
| UNS number | G41350 |
| US name | SAE 4137, SAE 4135H, SAE 4135, SAE 17-22-A S, ASTM L7M, ASTM L7B, ASTM G41370, ASTM G55, ASTM F70, ASTM F65, ASTM B1, ASTM 4137, ASTM 4130H, ASTM 4130, ~SAE 4130, ~ASTM H 70, ~ASTM H65, ~ASTM H55, ~ASTM G41300, ~ASTM G70, ~ASTM G65, ~ASTM 4130 |
| EN name | ~34CrMo4 |
| EN number | ~1.7226, ~1.722 |
| ISO name | 34CrMoS4, 33CrAlMo5-4, ~34CrMo4 |
MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey