| AISI 1030 Annealed Carbon Steel Mechanical Properties | Values |
|---|---|
| Young’s modulus | 208 – 216 GPa |
| Specific stiffness | 26.5 – 27.5 MN.m/kg |
| Yield strength (elastic limit) | 305 – 375 MPa |
| Tensile strength | 410 – 515 MPa |
| Specific strength | 38.8 – 47.8 kN.m/kg |
| Elongation | 25 – 38 % strain |
| Compressive strength | * 305 – 375 MPa |
| Flexural modulus | * 208 – 216 GPa |
| Flexural strength (modulus of rupture) | 305 – 375 MPa |
| Shear modulus | 80 – 85 GPa |
| Bulk modulus | 161 – 176 GPa |
| Poisson’s ratio | 0.285 – 0.295 |
| Shape factor | 59 |
| Hardness – Vickers | 120 – 145 HV |
| Elastic stored energy (springs) | 221 – 329 kJ/m^3 |
| Fatigue strength at 10^7 cycles | * 229 – 269 MPa |
| Fatigue strength model (stress range) | * 196 – 314 MPa |
| Fracture toughness | * 41 – 67 MPa.m^0.5 |
| Toughness (G) | 8.32 – 20.2 kJ/m^2 |