AISI 1020 Annealed vs As Rolled vs Normalized: Yield, Tensile & Hardness Compared

How do the AISI 1020 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1020 low carbon steel (UNS G10200) side by side for 3 conditions: annealed, as rolled, normalized. All values are taken from the individual AISI 1020 material data sheets linked below.

AISI 1020 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed265–325355–435110–13028–4345.7
As Rolled295–365395–500135–16528–4336.6
Normalized310–350395–490125–15028–4339.6

AISI 1020 Differences Compared with Annealed

The table below shows how much each AISI 1020 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+12%+13%+25%+0%
Normalized+12%+12%+15%+0%

AISI 1020 Strength and Hardness Charts

AISI 1020 Yield strength by condition (MPa)Annealed265–325As Rolled295–365Normalized310–350
AISI 1020 Tensile strength by condition (MPa)Annealed355–435As Rolled395–500Normalized395–490
AISI 1020 Hardness by condition (HV)Annealed110–130As Rolled135–165Normalized125–150

AISI 1020 Heat Treatment Key Points

The highest tensile strength of AISI 1020 in these data sheets is reached in the as rolled condition (395–500 MPa). The softest condition is annealed (110–130 HV), with a machining speed of 45.7 m/min, which is usually preferred for machining and forming.

AISI 1020 Material Data Sheets

AISI 1020 Annealed | AISI 1020 As Rolled | AISI 1020 Normalized | All AISI 1020 conditions

Looking for AISI 1020 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1020 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.