PPA General Purpose Grade Material Data Sheet

PPA General Purpose Grade (Polyphthalamide) Material Data Sheet

PPA General Purpose Grade Overview

PPA general purpose grade is a grade of polyphthalamide (PPA), designated Polyphthalamide (Unreinforced). This PPA general purpose grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.

PPA General Purpose Grade Designation

Polyphthalamide (Unreinforced)
TradenamesAkromid, Amodel, Arlen, Badamid, Durethan, Lubriloy, Novamid, Sepaz, Star-Therm, Tecomid, Terez, Tribocomp, Vampamid, Vestamid Htplus, Zytel

PPA General Purpose Grade Typical uses

Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications

PPA General Purpose Grade Composition detail

Polymer100  %

PPA General Purpose Grade Physical properties

Density1.13–1.15g/cm3

PPA General Purpose Grade Mechanical properties

Young’s modulus1.64–2.04GPa
Specific stiffness1.44–1.79MN.m/kg
Yield strength (elastic limit)44.3–55.2MPa
Tensile strength63–77.1MPa
Specific strength38.8–48.4kN.m/kg
Elongation24.6–35.4% strain
Elongation at yield8.63–16.4% strain
Compressive modulus1.75–1.93GPa
Compressive strength79.9–88.3MPa
Flexural modulus3–3.6GPa
Flexural strength (modulus of rupture)85.7–105MPa
Shear modulus0.641–0.674GPa
Shear strength37.8–46.2MPa
Bulk modulus2.85–3.15GPa
Poisson’s ratio0.383–0.398 
Shape factor4.5
Hardness – Vickers14–16HV
Hardness – Rockwell M121–133 
Hardness – Rockwell R121–133 
Hardness – Shore D83–86 
Elastic stored energy (springs)531–842kJ/m3
Fatigue strength at 10^7 cycles26.6–29.4MPa

PPA General Purpose Grade Impact & fracture properties

Fracture toughness3.46–3.82MPa.m0.5
Toughness (G)6.26–8.34kJ/m2
Impact strength, notched 23 °C13.8–26.8kJ/m2
Impact strength, notched -30 °C6.99–15.2kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PPA General Purpose Grade Thermal properties

Melting point299–322°C
Glass temperature119–135°C
Heat deflection temperature 0.45MPa126–166°C
Heat deflection temperature 1.8MPa101–140°C
Maximum service temperature108–124°C
Minimum service temperature-49–-29°C
Thermal conductivity0.2–0.25W/m.°C
Specific heat capacity1560–1620J/kg.°C
Thermal expansion coefficient90–95µstrain/°C
Thermal shock resistance251–341°C
Thermal distortion resistance0.00216–0.00271MW/m

PPA General Purpose Grade Electrical properties

Electrical resistivity1.64e20–4.1e21µohm.cm
Electrical conductivity4.21e-20–1.05e-18%IACS
Dielectric constant (relative permittivity)2.99–4.21 
Dissipation factor (dielectric loss tangent)0.0066–0.0174 
Dielectric strength (dielectric breakdown)12.6–21.4MV/m
Comparative tracking index600  V

PPA General Purpose Grade Magnetic properties

Magnetic typeNon-magnetic

PPA General Purpose Grade Optical, aesthetic and acoustic properties

TransparencyTranslucent
Acoustic velocity1200–1340m/s
Mechanical loss coefficient (tan delta)0.0138–0.0153 

PPA General Purpose Grade Absorption & permeability

Water absorption @ 24 hrs0.68–1.1%
Water absorption @ sat8.3–11%
Humidity absorption @ sat2.3–3.1%

PPA General Purpose Grade Processing properties

Polymer injection moldingExcellent
Polymer extrusionUnsuitable
Polymer thermoformingLimited use
Linear mold shrinkage1.5 – 2 %
Melt temperature268 – 349 °C
Molding pressure range34.4 – 103 MPa

PPA General Purpose Grade Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsLimited use
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsLimited use
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning