PPA Extra Tough Grade (Polyphthalamide) Material Data Sheet
PPA Extra Tough Grade Overview
PPA extra tough grade is a grade of polyphthalamide (PPA), designated Polyphthalamide (Extra tough). This PPA extra tough grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.
PPA Extra Tough Grade Designation
Polyphthalamide (Extra tough)
Tradenames
Amodel, Tecomid, Zytel
PPA Extra Tough Grade Typical uses
Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications
PPA Extra Tough Grade Composition detail
Polymer
75
–
85
%
Impact modifier
15
–
25
%
PPA Extra Tough Grade Physical properties
Density
1.1
–
1.12
g/cm3
PPA Extra Tough Grade Mechanical properties
Young’s modulus
2.05
–
2.55
GPa
Specific stiffness
1.85
–
2.3
MN.m/kg
Yield strength (elastic limit)
56.4
–
70.3
MPa
Tensile strength
68.4
–
83.6
MPa
Specific strength
50.8
–
63.4
kN.m/kg
Elongation
24.6
–
35.4
% strain
Elongation at yield
8.63
–
16.4
% strain
Compressive modulus
2.19
–
2.42
GPa
Compressive strength
86.6
–
95.8
MPa
Flexural modulus
2.09
–
2.51
GPa
Flexural strength (modulus of rupture)
65.7
–
80.3
MPa
Shear modulus
0.796
–
0.837
GPa
Shear strength
51.3
–
62.7
MPa
Bulk modulus
3.96
–
4.38
GPa
Poisson’s ratio
0.392
–
0.408
Shape factor
4.5
Hardness – Vickers
18
–
20
HV
Hardness – Rockwell M
126
–
139
Hardness – Rockwell R
126
–
139
Hardness – Shore D
84
–
88
Elastic stored energy (springs)
688
–
1090
kJ/m3
Fatigue strength at 10^7 cycles
28.9
–
31.9
MPa
PPA Extra Tough Grade Impact & fracture properties
Fracture toughness
3.62
–
4
MPa.m0.5
Toughness (G)
5.49
–
7.31
kJ/m2
Impact strength, notched 23 °C
66
–
128
kJ/m2
Impact strength, notched -30 °C
15.8
–
34.3
kJ/m2
Impact strength, unnotched 23 °C
590
–
600
kJ/m2
Impact strength, unnotched -30 °C
590
–
600
kJ/m2
PPA Extra Tough Grade Thermal properties
Melting point
299
–
322
°C
Glass temperature
119
–
135
°C
Heat deflection temperature 0.45MPa
126
–
166
°C
Heat deflection temperature 1.8MPa
101
–
140
°C
Maximum service temperature
108
–
124
°C
Minimum service temperature
-49
–
-29
°C
Thermal conductivity
0.255
–
0.265
W/m.°C
Specific heat capacity
1600
–
1660
J/kg.°C
Thermal expansion coefficient
58.3
–
60.7
µstrain/°C
Thermal shock resistance
397
–
539
°C
Thermal distortion resistance
0.00425
–
0.0045
MW/m
PPA Extra Tough Grade Electrical properties
Electrical resistivity
2e21
–
5e22
µohm.cm
Electrical conductivity
3.45e-21
–
8.62e-20
%IACS
Dielectric constant (relative permittivity)
2.99
–
4.21
Dissipation factor (dielectric loss tangent)
0.0066
–
0.0174
Dielectric strength (dielectric breakdown)
12.6
–
21.4
MV/m
Comparative tracking index
600
V
PPA Extra Tough Grade Magnetic properties
Magnetic type
Non-magnetic
PPA Extra Tough Grade Optical, aesthetic and acoustic properties