PA46 General Purpose Grade Material Data Sheet

PA46 General Purpose Grade (Polyamide 46) Material Data Sheet

PA46 General Purpose Grade Overview

PA46 general purpose grade is a grade of polyamide 46 (PA46, nylon 46), designated Polyamide (Nylon) (Type 46, Unreinforced). This PA46 general purpose grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA46 parts in-house and inspects them before shipment.

PA46 General Purpose Grade Designation

Polyamide (Nylon) (Type 46, Unreinforced)
TradenamesComco, Coolpoly, Hifill, Luvocom, Pentamid, Quadrant, Stanyl

PA46 General Purpose Grade Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA46 General Purpose Grade Composition detail

Polymer100  %

PA46 General Purpose Grade Physical properties

Density1.19–1.21g/cm3

PA46 General Purpose Grade Mechanical properties

Young’s modulus0.89–1.11GPa
Specific stiffness0.741–0.925MN.m/kg
Yield strength (elastic limit)48.1–60MPa
Tensile strength49.2–60.1MPa
Specific strength40.1–50kN.m/kg
Elongation22.9–33% strain
Elongation at yield13.5–25.6% strain
Compressive modulus0.95–1.05GPa
Compressive strength62.3–68.8MPa
Flexural modulus0.819–0.981GPa
Flexural strength (modulus of rupture)45–55MPa
Shear modulus0.348–0.366GPa
Shear strength29.5–36.1MPa
Bulk modulus1.6–1.77GPa
Poisson’s ratio0.385–0.401 
Shape factor3.4
Hardness – Vickers15–17HV
Hardness – Rockwell M105–116 
Hardness – Rockwell R105–116 
Hardness – Shore D79–82 
Elastic stored energy (springs)1150–1830kJ/m3
Fatigue strength at 10^7 cycles20.8–22.9MPa

PA46 General Purpose Grade Impact & fracture properties

Fracture toughness3.06–3.38MPa.m0.5
Toughness (G)9.01–12kJ/m2
Impact strength, notched 23 °C21.6–42kJ/m2
Impact strength, notched -30 °C14.9–32.5kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA46 General Purpose Grade Thermal properties

Melting point284–306°C
Glass temperature71–79°C
Heat deflection temperature 0.45MPa164–208°C
Heat deflection temperature 1.8MPa139–182°C
Maximum service temperature73–87°C
Minimum service temperature-58–-38°C
Thermal conductivity0.283–0.294W/m.°C
Specific heat capacity1550–1610J/kg.°C
Thermal expansion coefficient73.3–74.7µstrain/°C
Thermal shock resistance627–851°C
Thermal distortion resistance0.00381–0.00398MW/m

PA46 General Purpose Grade Electrical properties

Electrical resistivity6.01e16–1.5e18µohm.cm
Electrical conductivity1.15e-16–2.87e-15%IACS
Dielectric constant (relative permittivity)15.5–21.8 
Dissipation factor (dielectric loss tangent)0.328–0.865 
Dielectric strength (dielectric breakdown)11.9–20.3MV/m
Comparative tracking index450–500V

PA46 General Purpose Grade Magnetic properties

Magnetic typeNon-magnetic

PA46 General Purpose Grade Optical, aesthetic and acoustic properties

Refractive index1.62–1.64 
TransparencyOpaque
Acoustic velocity860–963m/s
Mechanical loss coefficient (tan delta)0.0265–0.0293 

PA46 General Purpose Grade Absorption & permeability

Water absorption @ 24 hrs2.6–4.3%
Water absorption @ sat11–15%
Humidity absorption @ sat3–4.1%

PA46 General Purpose Grade Processing properties

Polymer injection moldingAcceptable
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage1.8 – 2 %
Melt temperature242 – 316 °C
Mold temperature40 – 80 °C
Molding pressure range34.4 – 103 MPa

PA46 General Purpose Grade Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisUnacceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning