PA46 Extrusion Grade Material Data Sheet

PA46 Extrusion Grade (Polyamide 46) Material Data Sheet

PA46 Extrusion Grade Overview

PA46 extrusion grade is a grade of polyamide 46 (PA46, nylon 46), designated Polyamide (Nylon) (Type 46, Extrusion). This PA46 extrusion grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA46 parts in-house and inspects them before shipment.

PA46 Extrusion Grade Designation

Polyamide (Nylon) (Type 46, Extrusion)
TradenamesComco, Coolpoly, Hifill, Luvocom, Pentamid, Quadrant, Stanyl

PA46 Extrusion Grade Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA46 Extrusion Grade Composition detail

Polymer100  %

PA46 Extrusion Grade Physical properties

Density1.17–1.19g/cm3

PA46 Extrusion Grade Mechanical properties

Young’s modulus0.89–1.11GPa
Specific stiffness0.754–0.941MN.m/kg
Yield strength (elastic limit)49–61.1MPa
Tensile strength64.8–79.2MPa
Specific strength41.5–51.8kN.m/kg
Elongation41–59% strain
Elongation at yield24.1–45.8% strain
Compressive modulus0.95–1.05GPa
Compressive strength81.7–90.3MPa
Flexural modulus0.819–0.981GPa
Flexural strength (modulus of rupture)45–55MPa
Shear modulus0.345–0.362GPa
Shear strength38.9–47.5MPa
Bulk modulus1.86–2.06GPa
Poisson’s ratio0.399–0.415 
Shape factor3.41
Hardness – Vickers16–17HV
Hardness – Rockwell M122–135 
Hardness – Rockwell R122–135 
Hardness – Shore D83–87 
Elastic stored energy (springs)1190–1900kJ/m3
Fatigue strength at 10^7 cycles27.4–30.2MPa

PA46 Extrusion Grade Impact & fracture properties

Fracture toughness3.06–3.38MPa.m0.5
Toughness (G)9.01–12kJ/m2
Impact strength, notched 23 °C30.6–59.4kJ/m2
Impact strength, notched -30 °C14.9–32.5kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA46 Extrusion Grade Thermal properties

Melting point284–306°C
Glass temperature71–79°C
Heat deflection temperature 0.45MPa98–135°C
Heat deflection temperature 1.8MPa73–108°C
Maximum service temperature73–87°C
Minimum service temperature-58–-38°C
Thermal conductivity0.233–0.242W/m.°C
Specific heat capacity1630–1700J/kg.°C
Thermal expansion coefficient73.3–74.7µstrain/°C
Thermal shock resistance638–867°C
Thermal distortion resistance0.00314–0.00328MW/m

PA46 Extrusion Grade Electrical properties

Electrical resistivity2e14–5e15µohm.cm
Electrical conductivity3.45e-14–8.62e-13%IACS
Dielectric constant (relative permittivity)15.5–21.8 
Dissipation factor (dielectric loss tangent)0.328–0.865 
Dielectric strength (dielectric breakdown)11.1–18.9MV/m
Comparative tracking index400–450V

PA46 Extrusion Grade Magnetic properties

Magnetic typeNon-magnetic

PA46 Extrusion Grade Optical, aesthetic and acoustic properties

Refractive index1.62–1.64 
TransparencyOpaque
Acoustic velocity867–972m/s
Mechanical loss coefficient (tan delta)0.0265–0.0293 

PA46 Extrusion Grade Absorption & permeability

Water absorption @ 24 hrs2.6–4.3%
Water absorption @ sat11–15%
Humidity absorption @ sat3.1–4.3%

PA46 Extrusion Grade Processing properties

Polymer injection moldingAcceptable
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.6 %
Melt temperature293 – 310 °C
Mold temperature40 – 80 °C
Molding pressure range34.4 – 103 MPa

PA46 Extrusion Grade Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisUnacceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning