PA46 Super-Tough Grade Material Data Sheet

PA46 Super-Tough Grade (Polyamide 46) Material Data Sheet

PA46 Super-Tough Grade Overview

PA46 super-tough grade is a grade of polyamide 46 (PA46, nylon 46), designated Polyamide (Nylon) (Type 46, Super-tough). This PA46 super-tough grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA46 parts in-house and inspects them before shipment.

PA46 Super-Tough Grade Designation

Polyamide (Nylon) (Type 46, Super-tough)
TradenamesStanyl

PA46 Super-Tough Grade Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA46 Super-Tough Grade Composition detail

Polymer75–80%
Impact modifier20–25%

PA46 Super-Tough Grade Physical properties

Density1.08–1.11g/cm3

PA46 Super-Tough Grade Mechanical properties

Young’s modulus0.534–0.666GPa
Specific stiffness0.487–0.609MN.m/kg
Yield strength (elastic limit)40.1–50MPa
Tensile strength41.3–50.5MPa
Specific strength36.6–45.7kN.m/kg
Elongation29.3–42.2% strain
Elongation at yield17.3–32.8% strain
Compressive modulus0.57–0.63GPa
Compressive strength52.1–57.5MPa
Flexural modulus0.501–0.6GPa
Flexural strength (modulus of rupture)36–44MPa
Shear modulus0.207–0.217GPa
Shear strength24.8–30.3MPa
Bulk modulus1.12–1.24GPa
Poisson’s ratio0.399–0.415 
Shape factor3.1
Hardness – Vickers13–14HV
Hardness – Rockwell M95–105 
Hardness – Rockwell R95–105 
Hardness – Shore D75–79 
Elastic stored energy (springs)1330–2120kJ/m3
Fatigue strength at 10^7 cycles17.4–19.3MPa

PA46 Super-Tough Grade Impact & fracture properties

Fracture toughness2.76–3.05MPa.m0.5
Toughness (G)12.2–16.3kJ/m2
Impact strength, notched 23 °C88.4–172kJ/m2
Impact strength, notched -30 °C18.9–41.1kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA46 Super-Tough Grade Thermal properties

Melting point284–306°C
Glass temperature71–79°C
Heat deflection temperature 0.45MPa98–135°C
Heat deflection temperature 1.8MPa73–108°C
Maximum service temperature73–87°C
Minimum service temperature-58–-38°C
Thermal conductivity0.233–0.242W/m.°C
Specific heat capacity1630–1700J/kg.°C
Thermal expansion coefficient142–145µstrain/°C
Thermal shock resistance449–609°C
Thermal distortion resistance0.00162–0.00169MW/m

PA46 Super-Tough Grade Electrical properties

Electrical resistivity2e14–5e15µohm.cm
Electrical conductivity3.45e-14–8.62e-13%IACS
Dielectric constant (relative permittivity)11.6–16.4 
Dissipation factor (dielectric loss tangent)0.358–0.943 
Dielectric strength (dielectric breakdown)11.1–18.9MV/m
Comparative tracking index475–525V

PA46 Super-Tough Grade Magnetic properties

Magnetic typeNon-magnetic

PA46 Super-Tough Grade Optical, aesthetic and acoustic properties

Refractive index1.62–1.64 
TransparencyOpaque
Acoustic velocity697–781m/s
Mechanical loss coefficient (tan delta)0.0339–0.0375 

PA46 Super-Tough Grade Absorption & permeability

Water absorption @ 24 hrs2.3–3.7%
Water absorption @ sat9.5–13%
Humidity absorption @ sat2.5–3.4%

PA46 Super-Tough Grade Processing properties

Polymer injection moldingAcceptable
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage1.8 – 2 %
Melt temperature242 – 316 °C
Mold temperature40 – 80 °C
Molding pressure range34.4 – 103 MPa

PA46 Super-Tough Grade Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisUnacceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning