Home » PA (Polyamide / Nylon) » PA66 (Polyamide 66 / Nylon 66) » PA66 Carbon Filled Grades » PA66 30% Carbon Fiber Material Data Sheet
PA66 30% Carbon Fiber (Polyamide 66) Material Data Sheet
PA66 30% Carbon Fiber Overview
PA66 30% carbon fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 30% PAN Carbon Fiber, Conductive – EMI Shielding). This PA66 30% carbon fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.
PA66 30% Carbon Fiber Designation
Polyamide (Nylon) (Type 66, 30% PAN Carbon Fiber, Conductive – EMI Shielding) Tradenames Bestnyl, LNP Thermocomp, Luvocom, Novamid, Nylfor, Staramide, Star-Therm, Strator, Tecomid, Tribocomp, Wellamid
PA66 30% Carbon Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA66 30% Carbon Fiber Composition detail
Polymer 70 % Carbon (fiber) 30 %
PA66 30% Carbon Fiber Physical properties
PA66 30% Carbon Fiber Mechanical properties
Young’s modulus 17.8 – 22.2 GPa Specific stiffness 13.9 – 17.3 MN.m/kg Yield strength (elastic limit) 178 – 222 MPa Tensile strength 180 – 220 MPa Specific strength 139 – 173 kN.m/kg Elongation 2.46 – 3.54 % strain Elongation at yield 2.07 – 3.93 % strain Compressive modulus 19 – 21 GPa Compressive strength 228 – 252 MPa Flexural modulus 13.1 – 15.7 GPa Flexural strength (modulus of rupture) 203 – 248 MPa Shear modulus 7.34 – 7.72 GPa Shear strength 108 – 132 MPa Bulk modulus 18.4 – 20.3 GPa Poisson’s ratio 0.315 – 0.328 Shape factor 8.19 Hardness – Vickers 57 – 63 HV Hardness – Rockwell M 184 – 204 Hardness – Rockwell R 184 – 204 Hardness – Shore D 98 – 102 Elastic stored energy (springs) 788 – 1250 kJ/m3 Fatigue strength at 10^7 cycles 76 – 84 MPa
PA66 30% Carbon Fiber Impact & fracture properties
Fracture toughness 5.6 – 6.19 MPa.m0.5 Toughness (G) 1.51 – 2.01 kJ/m2 Impact strength, notched 23 °C 12.5 – 24.2 kJ/m2 Impact strength, notched -30 °C 8.85 – 19.2 kJ/m2 Impact strength, unnotched 23 °C 47.1 – 69.2 kJ/m2
PA66 30% Carbon Fiber Thermal properties
Melting point 258 – 265 °C Glass temperature 54 – 66 °C Heat deflection temperature 0.45MPa 260 – 266 °C Heat deflection temperature 1.8MPa 243 – 260 °C Maximum service temperature 90 – 130 °C Minimum service temperature -81 – -71 °C Thermal conductivity 0.97 – 1.05 W/m.°C Specific heat capacity 1410 – 1470 J/kg.°C Thermal expansion coefficient 19.8 – 28.8 µstrain/°C Thermal shock resistance 331 – 529 °C Thermal distortion resistance 0.0349 – 0.0511 MW/m
PA66 30% Carbon Fiber Electrical properties
Electrical resistivity 2e9 – 5e10 µohm.cm Electrical conductivity 3.45e-9 – 8.62e-8 %IACS Comparative tracking index 100 V Galvanic potential 0.14 – 0.22 V
PA66 30% Carbon Fiber Magnetic properties
Magnetic type Non-magnetic
PA66 30% Carbon Fiber Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3720 – 4170 m/s Mechanical loss coefficient (tan delta) 0.00662 – 0.00732
PA66 30% Carbon Fiber Absorption & permeability
Water absorption @ 24 hrs 0.51 – 0.83 % Water absorption @ sat 5 – 6.6 % Humidity absorption @ sat 1.4 – 1.8 %
PA66 30% Carbon Fiber Processing properties
Polymer injection molding Limited use Polymer extrusion Unsuitable Polymer thermoforming Limited use Linear mold shrinkage 0.1 – 0.3 % Melt temperature 220 – 310 °C Mold temperature 60 – 80 °C Molding pressure range 68.8 – 138 MPa
PA66 30% Carbon Fiber Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Acceptable Strong alkalis Acceptable Organic solvents Excellent Oxidation at 500C Unacceptable UV radiation (sunlight) Poor Flammability Slow-burning