C12500 Fire-Refined Tough-Pitch H.C. Copper, Soft Material Data Sheet
C12500 Fire-Refined Tough-Pitch H.C. Copper Material Data Sheet (Wrought, Soft)
C12500 Soft Copper Overview
C12500 soft copper is a wrought general purpose copper (UNS C12500, EN CW006A), known as fire-refined tough-pitch h.c. copper. Condition: Soft. This C12500 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C12500 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C12500 copper parts in-house and inspects them before shipment.
Architectural uses, kettles, stills, vats, gaskets, general electrical uses.
C12500 Soft Copper Composition detail
As (arsenic)
0
–
0.012
%
Bi (bismuth)
0
–
0.003
%
Cu (copper)
99.9
–
100
%
Ni (nickel)
0
–
0.05
%
Pb (lead)
0
–
0.004
%
Sb (antimony)
0
–
0.003
%
Se (selenium)
0
–
0.0125
%
Te (tellurium)
0
–
0.0125
%
C12500 Physical properties
Density
8.94
–
8.95
g/cm3
C12500 Soft Copper Mechanical properties
Young’s modulus
122
–
128
GPa
Specific stiffness
13.6
–
14.3
MN.m/kg
Yield strength (elastic limit)
45
–
55
MPa
Tensile strength
210
–
230
MPa
Specific strength
5.03
–
6.15
kN.m/kg
Elongation
46
–
50
% strain
Compressive strength
45
–
55
MPa
Flexural modulus
122
–
128
GPa
Flexural strength (modulus of rupture)
45
–
55
MPa
Shear modulus
44
–
46
GPa
Bulk modulus
132
–
138
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
46
–
56
HV
Elastic stored energy (springs)
8.17
–
12
kJ/m3
Fatigue strength at 10^7 cycles
70
–
80
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
67
–
83.6
MPa
C12500 Impact & fracture properties
Fracture toughness
92.7
–
97.4
MPa.m0.5
Toughness (G)
68.4
–
76.3
kJ/m2
C12500 Soft Copper Thermal properties
Melting point
1080
°C
Maximum service temperature
77
–
87
°C
Minimum service temperature
-273
°C
Thermal conductivity
331
–
372
W/m.°C
Specific heat capacity
379
–
382
J/kg.°C
Thermal expansion coefficient
16.8
–
16.9
µstrain/°C
Thermal shock resistance
21.3
–
26.2
°C
Thermal distortion resistance
19.6
–
22.1
MW/m
Latent heat of fusion
200
–
208
kJ/kg
C12500 Electrical properties
Electrical resistivity
1.82
–
1.95
µohm.cm
Electrical conductivity
88.4
–
94.7
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
C12500 Magnetic properties
Magnetic type
Non-magnetic
C12500 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3690
–
3780
m/s
Mechanical loss coefficient (tan delta)
0.00132
–
0.00198
C12500 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
30.5 m/min
Weldability Notes: Preheating and post weld heat treatment are not required
Good
C12500 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
C12500 Soft Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C12500 Notes
C12500 Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C12500 Standards with similar compositions
South Africa: 806 to SABS 806, 807 to SABS 807
UK: C106 to BS 2873
USA: C12500, C12510, C14530, C14530 to ASTM B152M, C14530 to ASTM B888, FRTP to ASTM B216, UNS C12500, UNS C12510, UNS C12700, UNS C12800, UNS C13000, UNS C14530