PPA 40% Mineral (Polyphthalamide) Material Data Sheet
PPA 40% Mineral Overview
PPA 40% mineral is a grade of polyphthalamide (PPA), designated Polyphthalamide (40% mineral). This PPA 40% mineral material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.
PPA 40% Mineral Designation
Polyphthalamide (40% mineral)
Tradenames
Amodel, Grivory, Tecomid
PPA 40% Mineral Typical uses
Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications
PPA 40% Mineral Composition detail
Polymer
60
%
Mineral (unspecified)
40
%
PPA 40% Mineral Physical properties
Density
1.53
–
1.57
g/cm3
PPA 40% Mineral Mechanical properties
Young’s modulus
7.46
–
9.3
GPa
Specific stiffness
4.81
–
6
MN.m/kg
Yield strength (elastic limit)
71.4
–
89.1
MPa
Tensile strength
86.7
–
106
MPa
Specific strength
46
–
57.5
kN.m/kg
Elongation
1.07
–
1.53
% strain
Elongation at yield
0.897
–
1.7
% strain
Compressive modulus
7.96
–
8.8
GPa
Compressive strength
110
–
121
MPa
Flexural modulus
6.28
–
7.52
GPa
Flexural strength (modulus of rupture)
159
–
195
MPa
Shear modulus
2.99
–
3.15
GPa
Shear strength
83.7
–
102
MPa
Bulk modulus
9.82
–
10.9
GPa
Poisson’s ratio
0.351
–
0.365
Shape factor
8.43
Hardness – Vickers
23
–
25
HV
Hardness – Rockwell M
142
–
157
Hardness – Rockwell R
142
–
157
Hardness – Shore D
88
–
92
Elastic stored energy (springs)
303
–
482
kJ/m3
Fatigue strength at 10^7 cycles
36.6
–
40.5
MPa
PPA 40% Mineral Impact & fracture properties
Fracture toughness
4.7
–
5.19
MPa.m0.5
Toughness (G)
2.54
–
3.38
kJ/m2
Impact strength, notched 23 °C
2.74
–
5.32
kJ/m2
Impact strength, notched -30 °C
1.89
–
4.11
kJ/m2
Impact strength, unnotched 23 °C
31.6
–
46.4
kJ/m2
Impact strength, unnotched -30 °C
24
–
36
kJ/m2
PPA 40% Mineral Thermal properties
Melting point
299
–
322
°C
Glass temperature
119
–
135
°C
Heat deflection temperature 0.45MPa
186
–
233
°C
Heat deflection temperature 1.8MPa
161
–
206
°C
Maximum service temperature
152
–
169
°C
Minimum service temperature
-49
–
-29
°C
Thermal conductivity
0.44
–
0.48
W/m.°C
Specific heat capacity
1290
–
1340
J/kg.°C
Thermal expansion coefficient
34
–
40
µstrain/°C
Thermal shock resistance
219
–
308
°C
Thermal distortion resistance
0.0114
–
0.0137
MW/m
PPA 40% Mineral Electrical properties
Electrical resistivity
1.5e20
–
3.76e21
µohm.cm
Electrical conductivity
4.59e-20
–
1.15e-18
%IACS
Dielectric constant (relative permittivity)
3.65
–
5.15
Dissipation factor (dielectric loss tangent)
0.00385
–
0.0102
Dielectric strength (dielectric breakdown)
18.7
–
31.9
MV/m
Comparative tracking index
550
–
600
V
PPA 40% Mineral Magnetic properties
Magnetic type
Non-magnetic
PPA 40% Mineral Optical, aesthetic and acoustic properties