PA69 Unfilled Grade Material Data Sheet

PA69 Unfilled Grade (Polyamide 69) Material Data Sheet

PA69 Unfilled Grade Overview

PA69 unfilled grade is a grade of polyamide 69 (PA69, nylon 69), designated Polyamide (Nylon) (Type 69, Molding and Extrusion). This PA69 unfilled grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA69 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA69 parts in-house and inspects them before shipment.

PA69 Unfilled Grade Designation

Polyamide (Nylon) (Type 69, Molding and Extrusion)
TradenamesAmilan; Antron; Aquanyl; Aramica; Ascend; Badamid; Bergamid; Bestnyl; Cordura; Dynacom; Emarex; Emmon; Ensiln; Ertalon; Esbrid; Estomid; Fostalink; Gapex; Grivory; Hiloy; Kobatron; Lubrilon; Lupon; Macromelt; Malecca; MCX-Q; NewNalon; Novamid; NSC; Nycast; Nylamid; Nylene; Nyloil; Nylube; Oilon; Oromid; Palmid; Polyslider; Ponamid; Pyronyl; Radiflam; Rayfan; Selar; Shinite; Spylon; StaMax; Starflam; Sunmide; Supplex; Tecast; Technystar; Terez; Texalon; Tismo Poticon; Trogamid; Tynex; Ultramid; Vekton; Wellamid; XTI; Zytel

PA69 Unfilled Grade Typical uses

General mechanical parts as for Nylon 6 or Nylon 66, but which require better dimensional stability.

PA69 Unfilled Grade Composition detail

Polymer100  %

PA69 Unfilled Grade Physical properties

Density1.08–1.1g/cm3

PA69 Unfilled Grade Mechanical properties

Young’s modulus1.85–1.94GPa
Specific stiffness1.69–1.78MN.m/kg
Yield strength (elastic limit)44.6–49.2MPa
Tensile strength55.8–61.5MPa
Specific strength40.9–45.2kN.m/kg
Elongation1050–1210% strain
Compressive modulus1.85–1.94GPa
Compressive strength66.8–73.8MPa
Flexural modulus1.95–2.04GPa
Flexural strength (modulus of rupture)78.1–86.1MPa
Shear modulus0.658–0.69GPa
Bulk modulus3.24–3.4GPa
Poisson’s ratio0.397–0.413 
Shape factor4.7
Hardness – Vickers13–15HV
Hardness – Rockwell M71–78 
Hardness – Rockwell R106–117 
Elastic stored energy (springs)526–639kJ/m3
Fatigue strength at 10^7 cycles20.6–26.7MPa

PA69 Unfilled Grade Impact & fracture properties

Fracture toughness1.59–2.32MPa.m0.5
Toughness (G)1.37–2.77kJ/m2
Impact strength, notched 23 °C5.5–6.1kJ/m2

PA69 Unfilled Grade Thermal properties

Melting point196–215°C
Glass temperature54–62°C
Heat deflection temperature 0.45MPa166–171°C
Heat deflection temperature 1.8MPa57–60°C
Maximum service temperature90–130°C
Minimum service temperature-62–-42°C
Thermal conductivity0.239–0.249W/m.°C
Specific heat capacity1500–1540J/kg.°C
Thermal expansion coefficient89.1–90.9µstrain/°C
Thermal shock resistance260–290°C
Thermal distortion resistance0.00265–0.00277MW/m

PA69 Unfilled Grade Electrical properties

Electrical resistivity1e19–1e21µohm.cm
Electrical conductivity1.72e-19–1.72e-17%IACS
Dielectric constant (relative permittivity)5.12–5.63 
Dissipation factor (dielectric loss tangent)0.019–0.021 
Dielectric strength (dielectric breakdown)22.7–24.6MV/m
Comparative tracking index250–600V

PA69 Unfilled Grade Magnetic properties

Magnetic typeNon-magnetic

PA69 Unfilled Grade Optical, aesthetic and acoustic properties

TransparencyTranslucent
Acoustic velocity1300–1340m/s
Mechanical loss coefficient (tan delta)0.0206–0.0216 

PA69 Unfilled Grade Absorption & permeability

Water absorption @ 24 hrs0.455–0.55%

PA69 Unfilled Grade Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage1 – 1.5 %
Melt temperature218 – 260 °C
Mold temperature40 – 80 °C
Molding pressure range6.88 – 103 MPa

PA69 Unfilled Grade Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisUnacceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning