Home » PA (Polyamide / Nylon) » PA6 (Polyamide 6 / Nylon 6) » PA6 Mineral Filled Grades » PA6 40% Mineral Material Data Sheet
PA6 40% Mineral (Polyamide 6) Material Data Sheet
PA6 40% Mineral Overview
PA6 40% mineral is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 40% Mineral). This PA6 40% mineral material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.
PA6 40% Mineral Designation
Polyamide (Nylon) (Type 6, 40% Mineral) Tradenames Adell, Altech, Chemlon, Denyl, Durethan, Lumid, Mazmid, Minlon, Nycal, Nymax, Pentamid, Scanamid, Staramide, Tarnamid, Ultramid, Wellamid
PA6 40% Mineral Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA6 40% Mineral Composition detail
Polymer 60 % Mineral (unspecified) 40 %
PA6 40% Mineral Physical properties
PA6 40% Mineral Mechanical properties
Young’s modulus 2.2 – 2.74 GPa Specific stiffness 1.49 – 1.86 MN.m/kg Yield strength (elastic limit) 49 – 61.1 MPa Tensile strength 52.2 – 63.8 MPa Specific strength 33.2 – 41.4 kN.m/kg Elongation 23 – 33 % strain Elongation at yield 11.7 – 22.3 % strain Compressive modulus 2.35 – 2.6 GPa Compressive strength 66.1 – 73.1 MPa Flexural modulus 1.87 – 2.23 GPa Flexural strength (modulus of rupture) 56.3 – 68.8 MPa Shear modulus 0.886 – 0.932 GPa Shear strength 31.3 – 38.3 MPa Bulk modulus 2.8 – 3.09 GPa Poisson’s ratio 0.34 – 0.36 Shape factor 5.01 Hardness – Vickers 16 – 17 HV Hardness – Rockwell M 109 – 120 Hardness – Rockwell R 109 – 120 Hardness – Brinell 80 – 100 HB Hardness – Shore D 80 – 83 Elastic stored energy (springs) 484 – 769 kJ/m3 Fatigue strength at 10^7 cycles 22 – 24.4 MPa
PA6 40% Mineral Impact & fracture properties
Fracture toughness 3.67 – 4.06 MPa.m0.5 Toughness (G) 5.25 – 7.01 kJ/m2 Impact strength, notched 23 °C 5.1 – 9.9 kJ/m2 Impact strength, notched -30 °C 2.52 – 5.48 kJ/m2 Impact strength, unnotched 23 °C 347 – 510 kJ/m2 Impact strength, unnotched -30 °C 66 – 99 kJ/m2
PA6 40% Mineral Thermal properties
Melting point 210 – 220 °C Glass temperature 44 – 56 °C Heat deflection temperature 0.45MPa 149 – 183 °C Heat deflection temperature 1.8MPa 132 – 141 °C Maximum service temperature 90 – 130 °C Minimum service temperature -64 – -54 °C Thermal conductivity 0.352 – 0.366 W/m.°C Specific heat capacity 1340 – 1400 J/kg.°C Thermal expansion coefficient 70.2 – 71.6 µstrain/°C Thermal shock resistance 270 – 366 °C Thermal distortion resistance 0.00496 – 0.00518 MW/m
PA6 40% Mineral Electrical properties
Electrical resistivity 2e20 – 5e21 µohm.cm Electrical conductivity 3.45e-20 – 8.62e-19 %IACS Dielectric constant (relative permittivity) 12.5 – 17.6 Dissipation factor (dielectric loss tangent) 0.138 – 0.363 Dielectric strength (dielectric breakdown) 28.1 – 47.9 MV/m Comparative tracking index 550 V
PA6 40% Mineral Magnetic properties
Magnetic type Non-magnetic
PA6 40% Mineral Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 1220 – 1370 m/s Mechanical loss coefficient (tan delta) 0.0176 – 0.0194
PA6 40% Mineral Absorption & permeability
Water absorption @ 24 hrs 1.1 – 1.8 % Water absorption @ sat 4.8 – 6.4 % Humidity absorption @ sat 1.5 – 2 %
PA6 40% Mineral Processing properties
Polymer injection molding Excellent Polymer extrusion Limited use Polymer thermoforming Limited use Linear mold shrinkage 0.3 – 0.6 % Melt temperature 192 – 288 °C Mold temperature 50 – 80 °C Molding pressure range 13.8 – 138 MPa
PA6 40% Mineral Durability
Water (fresh) Excellent Water (salt) Acceptable Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Limited use Strong alkalis Limited use Organic solvents Acceptable Oxidation at 500C Unacceptable UV radiation (sunlight) Fair Flammability Slow-burning
PA6 Grades
PA6 Mineral Filled Material Data Sheets
Mineral 40% Mineral You are here
All PA6 Grades