NIMONIC PE16 (bar) Material Data Sheet

Nickel-Fe-Cr alloy, NIMONIC PE16, bar

NIMONIC PE16 Designation

INCO Inc.Proprietary Alloy: “NIMONIC PE16”

NIMONIC PE16 Tradenames

NIMONIC PE16Special Metals Corp. (USA)

NIMONIC PE16 Typical uses

Aerospace

NIMONIC PE16 Composition detail

Al (aluminum)1  %
Cr (chromium)16.5  %
Fe (iron)34.4  %
Mo (molybdenum)3.2  %
Ni (nickel)43.5  %
Ti (titanium)1.2  %
Other0–0.1%

NIMONIC PE16 Physical properties

Density 7.95–8.1g/cm3

NIMONIC PE16 Mechanical properties

Young’s modulus195–205GPa
Specific stiffness24.3–25.6MN.m/kg
Yield strength (elastic limit)460–585MPa
Tensile strength795–975MPa
Specific strength57.3–72.9kN.m/kg
Elongation30–45% strain
Compressive strength460–585MPa
Flexural modulus195–205GPa
Flexural strength (modulus of rupture)460–585MPa
Shear modulus75–85GPa
Bulk modulus145–175GPa
Poisson’s ratio0.28–0.3 
Shape factor25   
Hardness – Vickers270–310HV
Hardness – Rockwell B103–106HRB
Hardness – Rockwell C26–31HRC
Hardness – Brinell256–294HB
Elastic stored energy (springs)536–846kJ/m3
Fatigue strength at 10^7 cycles315–490MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
294–525MPa

NIMONIC PE16 Impact & fracture properties

Fracture toughness215–239MPa.m0.5
Toughness (G)231–285kJ/m2

NIMONIC PE16 Thermal properties

Melting point1230–1380°C
Maximum service temperature697–967°C
Minimum service temperature-273  °C
Thermal conductivity11–12.5W/m.°C
Specific heat capacity525–565J/kg.°C
Thermal expansion coefficient10.5–12.5µstrain/°C
Thermal shock resistance195–262°C
Thermal distortion resistance0.92–1.14MW/m
Latent heat of fusion270–300kJ/kg

NIMONIC PE16 Electrical properties

Electrical resistivity105–115µohm.cm
Electrical conductivity1.5–1.64%IACS
Galvanic potential-0.13–-0.05V

NIMONIC PE16 Magnetic properties

Magnetic typeNon-magnetic

NIMONIC PE16 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity4930–5060m/s
Mechanical loss coefficient (tan delta)3e-4–5e-4 

NIMONIC PE16 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed5.79 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good

NIMONIC PE16 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Bronze or zinc alloy dies should be used to minimize galling.  
Limited use
FlammabilityNon-flammable

NIMONIC PE16 Corrosion resistance

Pitting resistance equivalent number (PREN)27.1
Pitting and crevice corrosionMedium (20-30)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydroxide
Slightly susceptible

NIMONIC PE16 Notes

Warning
All nickel compounds should be regarded as toxic.  Some can cause cancer and/or fetal abnormalities.
Other notes
NIMONIC is a registered tradename of the INCO group of companies.

NIMONIC PE16 Standards with similar compositions

Tradenames: NIMONIC PE 16

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey