INCOLOY 800 Material Data Sheet (Spring Temper, Wire)

Nickel-Fe-Cr alloy, INCOLOY 800, spring temper, wire

INCOLOY 800 Designation (spring temper, wire)

Unified Numbering System (USA): N08800
ConditionSpring temper
UNS numberN08800
US nameASTM Grade N08800; AMS 5766, 5871
EN nameX 10 NiCrAlTi 32 20
EN number1.4876
ISO nameISO 9723, 9724, 9725, 6207, 6208

INCOLOY 800 Tradenames (spring temper, wire)

INCOLOY 800Special Metals Corp. (USA)
AD NY810Aubert & Duval (FRANCE)

INCOLOY 800 Typical uses (spring temper, wire)

Heat treating equipment, petrochemical pyrolysis tubing and piping systems, sheathing for electrical heating elements, food processing equipment

INCOLOY 800 Composition detail (spring temper, wire)

Al (aluminum)0–1%
Cr (chromium)19–23%
Cu (copper)0–0.75%
Fe (iron)39.5–50%
Mn (manganese)0–1.5%
Ni (nickel)30–35%
Si (silicon)0–1%
Ti (titanium)0.15–0.6%
Other0–0.1%

INCOLOY 800 Physical properties (spring temper, wire)

Density7.85–8.05g/cm3

INCOLOY 800 Mechanical properties (spring temper, wire)

Young’s modulus190–200GPa
Specific stiffness23.8–25.2MN.m/kg
Yield strength (elastic limit)895–1180MPa
Tensile strength965–1210MPa
Specific strength113–148kN.m/kg
Elongation2–5% strain
Compressive strength895–1180MPa
Flexural modulus190–200GPa
Flexural strength (modulus of rupture)895–1180MPa
Shear modulus70–76GPa
Bulk modulus186–224GPa
Poisson’s ratio0.33–0.35 
Shape factor1   
Hardness – Vickers280–380HV
Hardness – Rockwell B103–111HRB
Hardness – Rockwell C27–39HRC
Hardness – Brinell265–360HB
Elastic stored energy (springs)2090–3490kJ/m3
Fatigue strength at 10^7 cycles385–605MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles358–651MPa

INCOLOY 800 Impact & fracture properties (spring temper, wire)

Fracture toughness24.3–27MPa.m0.5
Toughness (G)3.04–3.75kJ/m2

INCOLOY 800 Thermal properties (spring temper, wire)

Melting point1360–1390°C
Maximum service temperature777–977°C
Minimum service temperature-273  °C
Thermal conductivity11–12W/m.°C
Specific heat capacity490–515J/kg.°C
Thermal expansion coefficient13.5–15µstrain/°C
Thermal shock resistance319–428°C
Thermal distortion resistance0.755–0.864MW/m
Latent heat of fusion270–300kJ/kg

INCOLOY 800 Electrical properties (spring temper, wire)

Electrical resistivity92–100µohm.cm
Electrical conductivity1.72–1.87%IACS
Galvanic potential-0.23–-0.15V

INCOLOY 800 Magnetic properties (spring temper, wire)

Magnetic typeNon-magnetic

INCOLOY 800 Optical, aesthetic and acoustic properties (spring temper, wire)

TransparencyOpaque
Acoustic velocity4880–5020m/s
Mechanical loss coefficient (tan delta)1e-4–3e-4 

INCOLOY 800 Processing properties (spring temper, wire)

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed12.2 – 18.3 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGFair
Weldability – plasmaFair
Weldability – SAWFair
Weldability – TIGFair
BrazeabilityGood

INCOLOY 800 Durability (spring temper, wire)

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Bronze or zinc alloy dies should be used to minimize galling.
Limited use
FlammabilityNon-flammable

INCOLOY 800 Corrosion resistance (spring temper, wire)

Pitting resistance equivalent number (PREN)19 – 23
Pitting and crevice corrosionMedium (20-30)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: HydroxideNot susceptible
Intergranular (weld line) corrosionExcellent
Inorganic acidsExcellent
Organic acidsExcellent
AlkalisGood
Humidity / waterExcellent
Sea waterModerate
Sour oil and gasExcellent

INCOLOY 800 Notes (spring temper, wire)

Warning
All nickel compounds should be regarded as toxic.  Some can cause cancer and/or fetal abnormalities.
Other notes
INCOLOY is a registered tradename of the INCO group of companies.
As of September 1999 , INCONEL, INCOLOY, MONEL, NIMONIC, INCO-WELD, NILO, BRIGHTRAY, CORRONEL and UDIMET have become registered trademarks of Special Metals Corporation
Keywords
BS 3072, BS 3075, BS 3076 NA15

INCOLOY 800 Standards with similar compositions (spring temper, wire)

Japan: NCF 800 TF to JIS G3467, NCF800 to JIS G4901, NCF800 to JIS G4902, NCF800TB to JIS G4904, NCF800TP to JIS G4903
South Korea: Incoloy 800 to KS D 3750, NCF 800 to KS D 3531, NCF 800 to KS D 3532, NCF 800 TP to KS D 3758
USA: UNS N08800
Tradenames: ALLEGHENY TYPE 332, ESSHETE 800, ESSHETE 800L

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey