Bronze CuMn13Al8 Mechanical Properties (C95700, Cast Aluminum bronze)

DesignationCuMn13Al8
UNS numberC95700
ISO nameCuMn13Al8Fe3Ni3
JIS (Japanese) nameAlBz4

Mechanical properties: Bronze CuMn13Al8 Mechanical Properties (C95700, Cast Aluminum bronze)

Young’s modulus114–118GPa
Specific stiffness15.1–15.7MN.m/kg
Yield strength (elastic limit)280–340MPa
Tensile strength650–730MPa
Specific strength37.2–45.2kN.m/kg
Elongation18–35% strain
Compressive strength280–340MPa
Flexural modulus114–118GPa
Flexural strength (modulus of rupture)280–340MPa
Shear modulus42.2–43.7GPa
Bulk modulus123–127GPa
Poisson’s ratio0.34–0.35 
Shape factor24   
Hardness – Vickers160–210HV
Elastic stored energy (springs)341–494kJ/m^3
Fatigue strength at 10^7 cycles242–261MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles217–291MPa

Impact & fracture properties

Fracture toughness38.8–44.2MPa.m^0.5
Toughness (G)13–16.8kJ/m^2

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey