Aluminum, EN AC-48000, chill cast, T6 Material Data Sheet

Aluminum, EN AC-48000, chill cast, T6

Aluminum, EN AC-48000, chill cast, T6 Designation

EN AC-48000 (DIN EN 1706)
ConditionT6 (Solution heat-treated and artificially aged)
EN numberEN AC-48000 / EN AC-AlSi12CuNiMg

Aluminum, EN AC-48000, chill cast, T6 Typical uses

High strength alloy for the automotive industry: space frames, wheels, axle and differential housings, pump, meter, differential housings, intake manifolds, electronic cases, fuel pumps

Aluminum, EN AC-48000, chill cast, T6 Composition detail

Al (aluminum)80.4–87.2%
Cu (copper)0.8–1.5%
Fe (iron)0–0.7%
Mg (magnesium)0.8–1.5%
Mn (manganese)0–0.35%
Ni (nickel)0.7–1.3%
Si (silicon)10.5–13.5%
Ti (titanium)0–0.25%
Zn (zinc)0–0.35%
Other0–0.15%

Aluminum, EN AC-48000, chill cast, T6 Physical properties

Density2.65–2.71g/cm3

Aluminum, EN AC-48000, chill cast, T6 Mechanical properties

Young’s modulus70.6–73.4GPa
Specific stiffness26.3–27.4MN.m/kg
Yield strength (elastic limit)234–258MPa
Tensile strength266–294MPa
Specific strength87.2–96.3kN.m/kg
Elongation1–1.2% strain
Compressive strength228–252MPa
Flexural modulus70.6–73.4GPa
Flexural strength (modulus of rupture)240–264MPa
Shear modulus26.4–27.8GPa
Bulk modulus66.1–75.5GPa
Poisson’s ratio0.322–0.338 
Shape factor27   
Hardness – Vickers108–119HV
Elastic stored energy (springs)381–462kJ/m^3
Fatigue strength at 10^7 cycles100–116MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
95.5–122MPa

Aluminum, EN AC-48000, chill cast, T6 Impact & fracture properties

Fracture toughness18–20.5MPa.m0.5
Toughness (G)4.51–5.82kJ/m2

Aluminum, EN AC-48000, chill cast, T6 Thermal properties

Melting point549–626°C
Maximum service temperature170–200°C
Minimum service temperature-273  °C
Thermal conductivity130–165W/m.°C
Specific heat capacity944–982J/kg.°C
Thermal expansion coefficient19.5–20.5µstrain/°C
Thermal shock resistance161–181°C
Thermal distortion resistance6.48–8.28MW/m
Latent heat of fusion384–393kJ/kg

Aluminum, EN AC-48000, chill cast, T6 Electrical properties

Electrical resistivity3.8–7.1µohm.cm
Electrical conductivity24.3–45.4%IACS
Galvanic potential-0.73–-0.65V

Aluminum, EN AC-48000, chill cast, T6 Magnetic properties

Magnetic typeNon-magnetic

Aluminum, EN AC-48000, chill cast, T6 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5.13e3–5.24e3m/s
Mechanical loss coefficient (tan delta)0.01–0.09 

Aluminum, EN AC-48000, chill cast, T6 Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed61 m/min
Weldability
Notes: Preheating and post weld heat treatments are not required
Excellent

Aluminum, EN AC-48000, chill cast, T6 Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsExcellent
Strong acidsExcellent
Weak alkalisAcceptable
Strong alkalisUnacceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum alloys perform poorly when self-mated but can be processed without galling when mated with steels.  
Limited use
FlammabilityNon-flammable

Aluminum, EN AC-48000, chill cast, T6 Corrosion resistance of metals

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Halide, water
Susceptible

Aluminum, EN AC-48000, chill cast, T6 Standards with similar compositions

Austria: AlSi12CuMgNi to ONORM M3429
Belgium: AlSi12CuNi to NBN P21-101
Czech Republic: 424336 to CSN
Europe: EN AB-48000 to CEN EN 1676, EN AC-48000 to CEN EN 1706
France: A-S11UNG to NF A50-702
Hungary: OAlSi12CuNiMg to MSZ 2679
India: 46258 to IS 7793, 4685 to IS 202 or 617
Japan: AC8A to JIS H5202, AC8A.1 to JIS H2211, AC8A.2 to JIS H2211
Russia: AK12MMgN to GOST 1583, AL30 to GOST 2685
South Africa: Al-Si12NiMgCu to SABS 991
Spain: L-2550 to UNE 38-255, L-2551 to UNE 38-203, L-2551 to UNE 38-265
UK: LM13 to BS 1490
Tradenames: CALYPSO 82 N, CALYPSO 82 P

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey