AISI 4140 Annealed Mechanical Properties, Low alloy steel (4100 Series, Cr-Mo Alloyed, 0.40% C )

AISI 4140 Annealed Mechanical Properties, Low alloy steel (4100 Series, Cr-Mo Alloyed, 0.40% C )

AISI 4140
ConditionAnnealed
Young’s modulus208–216GPa
Specific stiffness26.5–27.5MN.m/kg
Yield strength (elastic limit)370–460MPa
Tensile strength595–720MPa
Specific strength47.1–58.6kN.m/kg
Elongation20–31% strain
Compressive strength370–460MPa
Flexural modulus208–216GPa
Flexural strength (modulus of rupture)370–460MPa
Shear modulus80–85GPa
Bulk modulus161–176GPa
Poisson’s ratio0.285–0.295 
Shape factor54   
Hardness – Vickers183–223HV
Elastic stored energy (springs)326–494kJ/m^3
Fatigue strength at 10^7 cycles297–341MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles261–389MPa
AISI 4140 Low alloy steel (4100 Series, Cr-Mo Alloyed, 0.40% C )
UNS numberG41400
US nameSAE H41400, SAE  4140, SAE 4142, SAE 4140, ASTM J  70, ASTM J  65, ASTM J  55, ASTM  4140, ASTM G41420, ASTM E7140, ASTM B7M, ASTM B16, ASTM 4142H, ASTM 4142, ASTM 4140H, ASTM 4140, ASTM 4137H, ASTM 41, ~SAE 4137H, ~ASTM B4D, ~ASTM 6
EN name~42CrMoS4, ~42CrMo4
EN number~1.7227, ~1.7223
ISO name~ 42 CrMoS 4, ~ 42 CrMo 4, ~42CrMo4
GB (Chinese) name~42CrMo
JIS (Japanese) nameSNB22-5, SNB22-4, SNB22-3, SNB22-2

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey