How do the AISI 1340 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1340 medium carbon manganese steel (UNS G13400, EN 38Mn6) side by side for 7 conditions: annealed, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C. All values are taken from the individual AISI 1340 material data sheets linked below.
AISI 1340 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) | Machining speed (m/min) |
|---|---|---|---|---|---|
| Annealed | 390–485 | 630–775 | 190–235 | 20–30 | 25.6 |
| Normalized | 500–615 | 750–925 | 230–280 | 17–27 | 21 |
| Oil Quenched & Tempered at 205°C | 1430–1760 | 1630–1990 | 455–555 | 8–14 | 9.75 |
| Oil Quenched & Tempered at 315°C | 1280–1570 | 1430–1750 | 408–498 | 9–15 | 11 |
| Oil Quenched & Tempered at 425°C | 1040–1270 | 1130–1400 | 340–415 | 11–17 | 13.7 |
| Oil Quenched & Tempered at 540°C | 740–915 | 865–1070 | 270–330 | 13–21 | 17.7 |
| Oil Quenched & Tempered at 650°C | 555–690 | 720–880 | 230–280 | 17–27 | 21.3 |
AISI 1340 Differences Compared with Annealed
The table below shows how much each AISI 1340 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| Normalized | +27% | +19% | +20% | -12% |
| Oil Quenched & Tempered at 205°C | +265% | +158% | +138% | -56% |
| Oil Quenched & Tempered at 315°C | +226% | +126% | +113% | -52% |
| Oil Quenched & Tempered at 425°C | +164% | +80% | +78% | -44% |
| Oil Quenched & Tempered at 540°C | +89% | +38% | +41% | -32% |
| Oil Quenched & Tempered at 650°C | +42% | +14% | +20% | -12% |
AISI 1340 Strength and Hardness Charts
AISI 1340 Heat Treatment Key Points
The highest tensile strength of AISI 1340 in these data sheets is reached in the oil quenched & tempered at 205°C condition (1630–1990 MPa). The softest condition is annealed (190–235 HV), with a machining speed of 25.6 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1340, raising the tempering temperature from 205°C to 650°C lowers hardness from 455–555 HV to 230–280 HV, trading strength for toughness and ductility.
AISI 1340 Material Data Sheets
AISI 1340 Annealed | AISI 1340 Normalized | AISI 1340 Oil Quenched & Tempered at 205°C | AISI 1340 Oil Quenched & Tempered at 315°C | AISI 1340 Oil Quenched & Tempered at 425°C | AISI 1340 Oil Quenched & Tempered at 540°C | AISI 1340 Oil Quenched & Tempered at 650°C | All AISI 1340 conditions
Looking for AISI 1340 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1340 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.