How do the AISI 1137 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1137 resulfurized medium carbon steel (UNS G11370) side by side for 13 conditions: annealed, as rolled, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C, water quenched & tempered at 205°C, water quenched & tempered at 315°C, water quenched & tempered at 425°C, water quenched & tempered at 540°C, water quenched & tempered at 650°C. All values are taken from the individual AISI 1137 material data sheets linked below.
AISI 1137 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) | Machining speed (m/min) |
|---|---|---|---|---|---|
| Annealed | 305–380 | 520–645 | 160–200 | 21–33 | 36.6 |
| As Rolled | 340–420 | 560–695 | 180–220 | 22–34 | 33.5 |
| Normalized | 355–435 | 595–740 | 185–225 | 18–27 | 30.5 |
| Oil Quenched & Tempered at 205°C | 840–1040 | 970–1200 | 320–390 | 4–6 | 17.7 |
| Oil Quenched & Tempered at 315°C | 755–930 | 885–1090 | 260–320 | 8–12 | 21 |
| Oil Quenched & Tempered at 425°C | 655–805 | 785–970 | 240–290 | 12–18 | 23.5 |
| Oil Quenched & Tempered at 540°C | 545–670 | 680–840 | 210–260 | 19–29 | 26.8 |
| Oil Quenched & Tempered at 650°C | 430–535 | 590–720 | 183–223 | 22–34 | 30.5 |
| Water Quenched & Tempered at 205°C | 1050–1290 | 1350–1650 | 375–455 | 4–6 | 14 |
| Water Quenched & Tempered at 315°C | 1010–1240 | 1230–1420 | 340–415 | 7–11 | 15.5 |
| Water Quenched & Tempered at 425°C | 885–1090 | 990–1220 | 280–350 | 11–17 | 18.9 |
| Water Quenched & Tempered at 540°C | 645–800 | 740–915 | 240–290 | 15–23 | 23.8 |
| Water Quenched & Tempered at 650°C | 475–590 | 580–715 | 173–213 | 20–30 | 33.5 |
AISI 1137 Differences Compared with Annealed
The table below shows how much each AISI 1137 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| As Rolled | +11% | +8% | +11% | +4% |
| Normalized | +15% | +15% | +14% | -17% |
| Oil Quenched & Tempered at 205°C | +174% | +86% | +97% | -81% |
| Oil Quenched & Tempered at 315°C | +146% | +70% | +61% | -63% |
| Oil Quenched & Tempered at 425°C | +113% | +51% | +47% | -44% |
| Oil Quenched & Tempered at 540°C | +77% | +30% | +31% | -11% |
| Oil Quenched & Tempered at 650°C | +41% | +12% | +13% | +4% |
| Water Quenched & Tempered at 205°C | +242% | +158% | +131% | -81% |
| Water Quenched & Tempered at 315°C | +228% | +127% | +110% | -67% |
| Water Quenched & Tempered at 425°C | +188% | +90% | +75% | -48% |
| Water Quenched & Tempered at 540°C | +111% | +42% | +47% | -30% |
| Water Quenched & Tempered at 650°C | +55% | +11% | +7% | -7% |
AISI 1137 Oil Quenched vs Water Quenched
Water removes heat faster than oil, so water quenched AISI 1137 forms more martensite and comes out harder and stronger, but with a higher risk of distortion and quench cracking. The table compares AISI 1137 oil quenched and water quenched material tempered at the same temperature, and shows the difference of water quenching relative to oil quenching (mid-points).
| Tempered at | Yield oil / water (MPa) | Yield diff. | Tensile oil / water (MPa) | Tensile diff. | Hardness oil / water (HV) | Hardness diff. |
|---|---|---|---|---|---|---|
| 205°C | 840–1040 / 1050–1290 | +24% | 970–1200 / 1350–1650 | +38% | 320–390 / 375–455 | +17% |
| 315°C | 755–930 / 1010–1240 | +34% | 885–1090 / 1230–1420 | +34% | 260–320 / 340–415 | +30% |
| 425°C | 655–805 / 885–1090 | +35% | 785–970 / 990–1220 | +26% | 240–290 / 280–350 | +19% |
| 540°C | 545–670 / 645–800 | +19% | 680–840 / 740–915 | +9% | 210–260 / 240–290 | +13% |
| 650°C | 430–535 / 475–590 | +10% | 590–720 / 580–715 | -1% | 183–223 / 173–213 | -5% |
AISI 1137 Strength and Hardness Charts
Oil quenched & tempered Water quenched & tempered. Dark bar = minimum, light bar = maximum of the range.
AISI 1137 Heat Treatment Key Points
The highest tensile strength of AISI 1137 in these data sheets is reached in the water quenched & tempered at 205°C condition (1350–1650 MPa). The softest condition is annealed (160–200 HV), with a machining speed of 36.6 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1137, raising the tempering temperature from 205°C to 650°C lowers hardness from 320–390 HV to 183–223 HV, trading strength for toughness and ductility. For water quenched AISI 1137, raising the tempering temperature from 205°C to 650°C lowers hardness from 375–455 HV to 173–213 HV, trading strength for toughness and ductility.
AISI 1137 is a resulfurized free-machining grade. See how it compares with the other free-machining steels in our resulfurized steels comparison.
AISI 1137 Material Data Sheets
AISI 1137 Annealed | AISI 1137 As Rolled | AISI 1137 Normalized | AISI 1137 Oil Quenched & Tempered at 205°C | AISI 1137 Oil Quenched & Tempered at 315°C | AISI 1137 Oil Quenched & Tempered at 425°C | AISI 1137 Oil Quenched & Tempered at 540°C | AISI 1137 Oil Quenched & Tempered at 650°C | AISI 1137 Water Quenched & Tempered at 205°C | AISI 1137 Water Quenched & Tempered at 315°C | AISI 1137 Water Quenched & Tempered at 425°C | AISI 1137 Water Quenched & Tempered at 540°C | AISI 1137 Water Quenched & Tempered at 650°C | All AISI 1137 conditions
Looking for AISI 1137 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1137 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.