PA410 Molding and Extrusion (Polyamide 410) Material Data Sheet
PA410 Molding and Extrusion Overview
PA410 molding and extrusion is a grade of polyamide 410 (PA410, nylon 410), designated Polyamide (Nylon) (Type 410). This PA410 molding and extrusion material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA410 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA410 parts in-house and inspects them before shipment.
PA410 Molding and Extrusion Impact & fracture properties
Fracture toughness
3.23
–
3.91
MPa.m0.5
Toughness (G)
6.41
–
9.26
kJ/m2
Impact strength, notched 23 °C
13
–
20
kJ/m2
Impact strength, notched -30 °C
3.5
–
3.6
kJ/m2
Impact strength, unnotched 23 °C
590
–
600
kJ/m2
Impact strength, unnotched -30 °C
590
–
600
kJ/m2
PA410 Molding and Extrusion Thermal properties
Melting point
250
°C
Glass temperature
52.3
–
66.3
°C
Heat deflection temperature 0.45MPa
165
–
185
°C
Heat deflection temperature 1.8MPa
67
–
87
°C
Vicat softening point
182
–
202
°C
Maximum service temperature
192
–
210
°C
Minimum service temperature
-64
–
-54
°C
Thermal conductivity
0.231
–
0.25
W/m.°C
Specific heat capacity
1430
–
1480
J/kg.°C
Thermal expansion coefficient
70
–
90
µstrain/°C
Thermal shock resistance
394
–
529
°C
Thermal distortion resistance
0.00266
–
0.00345
MW/m
PA410 Molding and Extrusion Electrical properties
Electrical resistivity
1e20
µohm.cm
Electrical conductivity
1.72e-18 %IACS
Dielectric constant (relative permittivity)
5.16
–
5.59
Dissipation factor (dielectric loss tangent)
0.208
–
0.3
Dielectric strength (dielectric breakdown)
28.6
–
31.5
MV/m
Comparative tracking index
571
–
630
V
PA410 Molding and Extrusion Magnetic properties
Magnetic type
Non-magnetic
PA410 Molding and Extrusion Optical, aesthetic and acoustic properties
Transparency
Transparent
Acoustic velocity
1210
–
1240
m/s
Mechanical loss coefficient (tan delta)
0.018
–
0.0238
PA410 Molding and Extrusion Absorption & permeability
Water absorption @ 24 hrs
0.505
–
0.611
%
Water absorption @ sat
5.27
–
6.38
%
Humidity absorption @ sat
1.9
–
2
%
Water vapor transmission
0.958
–
1.73
g.mm/m².day
Permeability (O2)
0.622
–
1.15
cm³.mm/m².day.atm
PA410 Molding and Extrusion Processing properties
First commercial production
2010
Polymer injection molding
Excellent
Polymer extrusion
Acceptable
Polymer thermoforming
Limited use
Linear mold shrinkage
1.2 – 1.3 %
Melt temperature
270 – 300 °C
Mold temperature
60 – 100 °C
PA410 Molding and Extrusion Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oils and fuels
Excellent
Oxidation at 500C
Unacceptable
UV radiation (sunlight)
Fair
Flammability
Slow-burning
PA410 Molding and Extrusion Notes
PA410 Molding and Extrusion Other notes
Polyamide 410 is 70% derived from castor oil. It has excellent mechanical properties, high heat stability and outstanding chemical resistance. Polyamide 410 also offers low permeability to both oxygen and water vapor; and and low moisture absorption for improved dimensional stability post conditioning. The impact modified grades offer improved impact resistance making them suitable for sports and leisure applications.