PA612 30% Glass Fiber 15% PTFE Lubricated Material Data Sheet

PA612 30% Glass Fiber 15% PTFE Lubricated (Polyamide 612) Material Data Sheet

PA612 30% Glass Fiber 15% PTFE Lubricated Overview

PA612 30% glass fiber 15% PTFE lubricated is a grade of polyamide 612 (PA612, nylon 612), designated Polyamide (Nylon) (Type 612, 15% PTFE/30% Glass Fiber Lubricated). This PA612 30% glass fiber 15% PTFE lubricated material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA612 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA612 parts in-house and inspects them before shipment.

PA612 30% Glass Fiber 15% PTFE Lubricated Designation

Polyamide (Nylon) (Type 612, 15% PTFE/30% Glass Fiber Lubricated)
TradenamesInlube, LNP Lubricomp, Tribocomp

PA612 30% Glass Fiber 15% PTFE Lubricated Typical uses

Mechanical parts, zips, filaments, coverings and coatings requiring abrasion resistance.

PA612 30% Glass Fiber 15% PTFE Lubricated Composition detail

Polymer55  %
PTFE (lubricant)15  %
Glass (fiber)30  %

PA612 30% Glass Fiber 15% PTFE Lubricated Physical properties

Density1.41–1.44g/cm3

PA612 30% Glass Fiber 15% PTFE Lubricated Mechanical properties

Young’s modulus6.33–7.9GPa
Specific stiffness4.44–5.55MN.m/kg
Yield strength (elastic limit)122–152MPa
Tensile strength123–150MPa
Specific strength85.6–107kN.m/kg
Elongation2.98–4.29% strain
Elongation at yield2.51–4.76% strain
Compressive modulus6.76–7.47GPa
Compressive strength156–172MPa
Flexural modulus5.67–6.79GPa
Flexural strength (modulus of rupture)183–224MPa
Shear modulus2.54–2.67GPa
Shear strength73.9–90.3MPa
Bulk modulus8.54–9.43GPa
Poisson’s ratio0.354–0.368 
Shape factor5.42
Hardness – Vickers39–43HV
Hardness – Rockwell M169–186 
Hardness – Rockwell R169–186 
Hardness – Shore D95–99 
Elastic stored energy (springs)1040–1650kJ/m3
Fatigue strength at 10^7 cycles52–57.5MPa

PA612 30% Glass Fiber 15% PTFE Lubricated Impact & fracture properties

Fracture toughness4.55–5.03MPa.m0.5
Toughness (G)2.8–3.74kJ/m2
Impact strength, notched 23 °C10.2–19.8kJ/m2
Impact strength, notched -30 °C6.3–13.7kJ/m2
Impact strength, unnotched 23 °C64.8–95.2kJ/m2
Impact strength, unnotched -30 °C42–63kJ/m2

PA612 30% Glass Fiber 15% PTFE Lubricated Thermal properties

Melting point195–217°C
Glass temperature40–52°C
Heat deflection temperature 0.45MPa199–247°C
Heat deflection temperature 1.8MPa174–220°C
Maximum service temperature90–120°C
Minimum service temperature-127–-107°C
Thermal conductivity0.436–0.453W/m.°C
Specific heat capacity1350–1410J/kg.°C
Thermal expansion coefficient31.7–33.1µstrain/°C
Thermal shock resistance510–693°C
Thermal distortion resistance0.0133–0.0141MW/m

PA612 30% Glass Fiber 15% PTFE Lubricated Electrical properties

Electrical resistivity2.73e21–6.83e22µohm.cm
Electrical conductivity2.52e-21–6.32e-20%IACS
Dielectric constant (relative permittivity)4.57–6.44 
Dissipation factor (dielectric loss tangent)0.0223–0.0587 
Dielectric strength (dielectric breakdown)20.4–34.7MV/m
Comparative tracking index600  V

PA612 30% Glass Fiber 15% PTFE Lubricated Magnetic properties

Magnetic typeNon-magnetic

PA612 30% Glass Fiber 15% PTFE Lubricated Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2100–2360m/s
Mechanical loss coefficient (tan delta)0.0101–0.0111 

PA612 30% Glass Fiber 15% PTFE Lubricated Absorption & permeability

Water absorption @ 24 hrs0.3–0.48%
Water absorption @ sat1.3–1.7%
Humidity absorption @ sat0.55–0.75%

PA612 30% Glass Fiber 15% PTFE Lubricated Processing properties

Polymer injection moldingExcellent
Polymer extrusionUnsuitable
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.3 %
Melt temperature213 – 288 °C
Mold temperature30 – 60 °C
Molding pressure range27.5 – 138 MPa

PA612 30% Glass Fiber 15% PTFE Lubricated Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning