PA6 40% Glass Fiber and Mineral Material Data Sheet

PA6 40% Glass Fiber and Mineral (Polyamide 6) Material Data Sheet

PA6 40% Glass Fiber and Mineral Overview

PA6 40% glass fiber and mineral is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 40% Glass Fiber and Mineral). This PA6 40% glass fiber and mineral material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 40% Glass Fiber and Mineral Designation

Polyamide (Nylon) (Type 6, 40% Glass Fiber and Mineral)
TradenamesAkulon, Akulon Ultraflow, Alcom, Ashlene, Bestnyl, Chemlon, Durethan, Grilon, Hylon, Lumid, Minlon, Nycal, Nymax, Pentamid, Radici, Scanamid, Schulamid, Slovamid, Tarnamid, Ultramid, Wellamid

PA6 40% Glass Fiber and Mineral Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 40% Glass Fiber and Mineral Composition detail

Polymer60  %
Glass (fiber)10–30%
Mineral (unspecified)10–30%

PA6 40% Glass Fiber and Mineral Physical properties

Density1.43–1.45g/cm3

PA6 40% Glass Fiber and Mineral Mechanical properties

Young’s modulus4.28–5.33GPa
Specific stiffness2.97–3.7MN.m/kg
Yield strength (elastic limit)60–74.8MPa
Tensile strength60.7–74.2MPa
Specific strength41.7–52kN.m/kg
Elongation5–7.19% strain
Elongation at yield4.2–7.98% strain
Compressive modulus4.56–5.05GPa
Compressive strength76.9–85MPa
Flexural modulus3.87–4.63GPa
Flexural strength (modulus of rupture)113–138MPa
Shear modulus1.72–1.81GPa
Shear strength36.4–44.5MPa
Bulk modulus5.43–6.01GPa
Poisson’s ratio0.34–0.36 
Shape factor6.6
Hardness – Vickers19–21HV
Hardness – Rockwell M118–130 
Hardness – Rockwell R118–130 
Hardness – Brinell85–105HB
Hardness – Shore D82–86 
Elastic stored energy (springs)373–592kJ/m3
Fatigue strength at 10^7 cycles25.6–28.3MPa

PA6 40% Glass Fiber and Mineral Impact & fracture properties

Fracture toughness4.2–4.64MPa.m0.5
Toughness (G)3.53–4.71kJ/m2
Impact strength, notched 23 °C5.74–11.1kJ/m2
Impact strength, notched -30 °C2.66–5.77kJ/m2
Impact strength, unnotched 23 °C51.6–75.9kJ/m2
Impact strength, unnotched -30 °C34.9–52.3kJ/m2

PA6 40% Glass Fiber and Mineral Thermal properties

Melting point210–220°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa210–218°C
Heat deflection temperature 1.8MPa199–207°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.451–0.469W/m.°C
Specific heat capacity1330–1380J/kg.°C
Thermal expansion coefficient19.8–73.8µstrain/°C
Thermal shock resistance189–714°C
Thermal distortion resistance0.00623–0.0232MW/m

PA6 40% Glass Fiber and Mineral Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)10.8–15.2 
Dissipation factor (dielectric loss tangent)0.138–0.365 
Dielectric strength (dielectric breakdown)22.5–38.3MV/m
Comparative tracking index400–550V

PA6 40% Glass Fiber and Mineral Magnetic properties

Magnetic typeNon-magnetic

PA6 40% Glass Fiber and Mineral Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1720–1930m/s
Mechanical loss coefficient (tan delta)0.0122–0.0135 

PA6 40% Glass Fiber and Mineral Absorption & permeability

Water absorption @ 24 hrs1.2–1.9%
Water absorption @ sat5.2–6.8%
Humidity absorption @ sat1.5–2%

PA6 40% Glass Fiber and Mineral Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.3 – 0.6 %
Melt temperature192 – 288 °C
Mold temperature60 – 90 °C
Molding pressure range13.8 – 138 MPa

PA6 40% Glass Fiber and Mineral Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning