PA6 40% Mineral Material Data Sheet

PA6 40% Mineral (Polyamide 6) Material Data Sheet

PA6 40% Mineral Overview

PA6 40% mineral is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 40% Mineral). This PA6 40% mineral material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 40% Mineral Designation

Polyamide (Nylon) (Type 6, 40% Mineral)
TradenamesAdell, Altech, Chemlon, Denyl, Durethan, Lumid, Mazmid, Minlon, Nycal, Nymax, Pentamid, Scanamid, Staramide, Tarnamid, Ultramid, Wellamid

PA6 40% Mineral Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 40% Mineral Composition detail

Polymer60  %
Mineral (unspecified)40  %

PA6 40% Mineral Physical properties

Density1.46–1.49g/cm3

PA6 40% Mineral Mechanical properties

Young’s modulus2.2–2.74GPa
Specific stiffness1.49–1.86MN.m/kg
Yield strength (elastic limit)49–61.1MPa
Tensile strength52.2–63.8MPa
Specific strength33.2–41.4kN.m/kg
Elongation23–33% strain
Elongation at yield11.7–22.3% strain
Compressive modulus2.35–2.6GPa
Compressive strength66.1–73.1MPa
Flexural modulus1.87–2.23GPa
Flexural strength (modulus of rupture)56.3–68.8MPa
Shear modulus0.886–0.932GPa
Shear strength31.3–38.3MPa
Bulk modulus2.8–3.09GPa
Poisson’s ratio0.34–0.36 
Shape factor5.01
Hardness – Vickers16–17HV
Hardness – Rockwell M109–120 
Hardness – Rockwell R109–120 
Hardness – Brinell80–100HB
Hardness – Shore D80–83 
Elastic stored energy (springs)484–769kJ/m3
Fatigue strength at 10^7 cycles22–24.4MPa

PA6 40% Mineral Impact & fracture properties

Fracture toughness3.67–4.06MPa.m0.5
Toughness (G)5.25–7.01kJ/m2
Impact strength, notched 23 °C5.1–9.9kJ/m2
Impact strength, notched -30 °C2.52–5.48kJ/m2
Impact strength, unnotched 23 °C347–510kJ/m2
Impact strength, unnotched -30 °C66–99kJ/m2

PA6 40% Mineral Thermal properties

Melting point210–220°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa149–183°C
Heat deflection temperature 1.8MPa132–141°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.352–0.366W/m.°C
Specific heat capacity1340–1400J/kg.°C
Thermal expansion coefficient70.2–71.6µstrain/°C
Thermal shock resistance270–366°C
Thermal distortion resistance0.00496–0.00518MW/m

PA6 40% Mineral Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)12.5–17.6 
Dissipation factor (dielectric loss tangent)0.138–0.363 
Dielectric strength (dielectric breakdown)28.1–47.9MV/m
Comparative tracking index550  V

PA6 40% Mineral Magnetic properties

Magnetic typeNon-magnetic

PA6 40% Mineral Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1220–1370m/s
Mechanical loss coefficient (tan delta)0.0176–0.0194 

PA6 40% Mineral Absorption & permeability

Water absorption @ 24 hrs1.1–1.8%
Water absorption @ sat4.8–6.4%
Humidity absorption @ sat1.5–2%

PA6 40% Mineral Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.3 – 0.6 %
Melt temperature192 – 288 °C
Mold temperature50 – 80 °C
Molding pressure range13.8 – 138 MPa

PA6 40% Mineral Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning