PA6 30% Carbon Fiber Material Data Sheet

PA6 30% Carbon Fiber (Polyamide 6) Material Data Sheet

PA6 30% Carbon Fiber Overview

PA6 30% carbon fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 30% PAN Carbon Fiber, Conductive – EMI Shielding). This PA6 30% carbon fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 30% Carbon Fiber Designation

Polyamide (Nylon) (Type 6, 30% PAN Carbon Fiber, Conductive – EMI Shielding)
TradenamesElectrafil, Hifill, Luvocom, Nylfor, Star-Therm, Tarnamid

PA6 30% Carbon Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 30% Carbon Fiber Composition detail

Polymer70  %
Carbon (fiber)30  %

PA6 30% Carbon Fiber Physical properties

Density1.26–1.28g/cm3

PA6 30% Carbon Fiber Mechanical properties

Young’s modulus12.9–16.1GPa
Specific stiffness10.2–12.7MN.m/kg
Yield strength (elastic limit)131–163MPa
Tensile strength132–162MPa
Specific strength103–128kN.m/kg
Elongation3.01–4.33% strain
Elongation at yield2.53–4.81% strain
Compressive modulus13.8–15.3GPa
Compressive strength168–185MPa
Flexural modulus10.1–12.1GPa
Flexural strength (modulus of rupture)185–226MPa
Shear modulus5.21–5.48GPa
Shear strength79.4–97MPa
Bulk modulus16.5–18.2GPa
Poisson’s ratio0.34–0.36 
Shape factor8.13
Hardness – Vickers42–46HV
Hardness – Rockwell M174–193 
Hardness – Rockwell R174–193 
Hardness – Shore D96–100 
Elastic stored energy (springs)588–933kJ/m3
Fatigue strength at 10^7 cycles55.9–61.7MPa

PA6 30% Carbon Fiber Impact & fracture properties

Fracture toughness5.25–5.81MPa.m0.5
Toughness (G)1.83–2.45kJ/m2
Impact strength, notched 23 °C6.77–13.1kJ/m2

PA6 30% Carbon Fiber Thermal properties

Melting point210–220°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa218–263°C
Heat deflection temperature 1.8MPa213–254°C
Maximum service temperature120–150°C
Minimum service temperature-64–-54°C
Thermal conductivity0.594–0.618W/m.°C
Specific heat capacity1470–1530J/kg.°C
Thermal expansion coefficient24.7–25.7µstrain/°C
Thermal shock resistance345–469°C
Thermal distortion resistance0.0234–0.0248MW/m

PA6 30% Carbon Fiber Electrical properties

Electrical resistivity2e8–5e9µohm.cm
Electrical conductivity3.45e-8–8.62e-7%IACS
Galvanic potential0.14–0.22V

PA6 30% Carbon Fiber Magnetic properties

Magnetic typeNon-magnetic

PA6 30% Carbon Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3180–3570m/s
Mechanical loss coefficient (tan delta)0.00756–0.00835 

PA6 30% Carbon Fiber Absorption & permeability

Water absorption @ 24 hrs0.72–1.2%
Water absorption @ sat5.8–7.8%
Humidity absorption @ sat2–2.6%

PA6 30% Carbon Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.1 – 0.3 %
Melt temperature222 – 302 °C
Mold temperature60 – 90 °C
Molding pressure range68.8 – 138 MPa

PA6 30% Carbon Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning