PA6 Molding and Extrusion (Polyamide 6) Material Data Sheet
PA6 Molding and Extrusion Overview
| PA6 molding and extrusion is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, Molding and Extrusion). This PA6 molding and extrusion material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment. |
PA6 Molding and Extrusion Designation
| Polyamide (Nylon) (Type 6, Molding and Extrusion) | |
| Tradenames | 4Mid, Addinyl, Aegis, Akromid, Akulon, Akulon Ultraflow, Alcom, Alphalon, Altech, Amilan, Anjacom, Anjamid, Aquamid, Armamid, Ashlene, Astamid, Badamid, Bergamid, Bestnyl, Capran, Capran Medallion, Chemlon, Clariant, Comco, Compamid, Denyl, Deslon, Dinalon, Distrumid, Domamid, Durethan, Dynacom, Ecotan, Eplamid, Germamid, Glamide, Gravi-Tech, Grilon, Heramid, Hifill, Hylon, Hylonselect, Isocor, Kepamid, Kopa, Lamigamid, LNP Thermocomp, Lumid, Luvocom, Mazmid, Miramid, Next Industrial, Next Prime, Nilamid, Niretan, Novamid, Novamide, Nybex, Nycal, Nycast, Nylaforce, Nylamid, Nylene, Nylfor, Nymax, Nypol, Nyrim, Orgalloy, Pentamid, Plustek, Polybest, Promyde, Pryme, Quadrant, Radici, Radilon, Scanamid, Schulamid, Selar, Shokamid, Silamid, Slovamid, Staramide, Tarnamid, Taromid, Technamid, Technyl, Technyl Star, Tekamid, Tekumid, Terez, Thermocomp, Thermylon, Tufnyl, Ultramid, Unitika, Venyl, Vitamide, Wellamid, Zytel |
PA6 Molding and Extrusion Typical uses
| Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils. |
PA6 Molding and Extrusion Composition detail
| Polymer | 100 | % |
PA6 Molding and Extrusion Physical properties
| Density | 1.13 | – | 1.15 | g/cm3 |
PA6 Molding and Extrusion Mechanical properties
| Young’s modulus | 0.944 | – | 1.18 | GPa |
| Specific stiffness | 0.828 | – | 1.04 | MN.m/kg |
| Yield strength (elastic limit) | 38.6 | – | 48.2 | MPa |
| Tensile strength | 32.9 | – | 40.2 | MPa |
| Specific strength | 33.9 | – | 42.3 | kN.m/kg |
| Elongation | 41 | – | 59 | % strain |
| Elongation at yield | 14.6 | – | 27.7 | % strain |
| Compressive modulus | 1.01 | – | 1.11 | GPa |
| Compressive strength | 41.6 | – | 46 | MPa |
| Flexural modulus | 0.77 | – | 0.923 | GPa |
| Flexural strength (modulus of rupture) | 43.2 | – | 52.7 | MPa |
| Shear modulus | 0.38 | – | 0.4 | GPa |
| Shear strength | 19.7 | – | 24.1 | MPa |
| Bulk modulus | 1.2 | – | 1.33 | GPa |
| Poisson’s ratio | 0.34 | – | 0.36 | |
| Shape factor | 3.79 | |||
| Hardness – Vickers | 12 | – | 14 | HV |
| Hardness – Rockwell M | 83 | – | 92 | |
| Hardness – Rockwell R | 83 | – | 92 | |
| Hardness – Shore D | 71 | – | 74 | |
| Elastic stored energy (springs) | 698 | – | 1110 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 13.9 | – | 15.3 | MPa |
PA6 Molding and Extrusion Impact & fracture properties
| Fracture toughness | 3.1 | – | 3.42 | MPa.m0.5 |
| Toughness (G) | 8.7 | – | 11.6 | kJ/m2 |
| Impact strength, notched 23 °C | 45.5 | – | 88.3 | kJ/m2 |
| Impact strength, notched -30 °C | 3.62 | – | 7.87 | kJ/m2 |
| Impact strength, unnotched 23 °C | 590 | – | 600 | kJ/m2 |
| Impact strength, unnotched -30 °C | 590 | – | 600 | kJ/m2 |
PA6 Molding and Extrusion Thermal properties
| Melting point | 210 | – | 220 | °C |
| Glass temperature | 44 | – | 56 | °C |
| Heat deflection temperature 0.45MPa | 175 | – | 191 | °C |
| Heat deflection temperature 1.8MPa | 68 | – | 85 | °C |
| Maximum service temperature | 90 | – | 130 | °C |
| Minimum service temperature | -64 | – | -54 | °C |
| Thermal conductivity | 0.233 | – | 0.253 | W/m.°C |
| Specific heat capacity | 1480 | – | 1520 | J/kg.°C |
| Thermal expansion coefficient | 144 | – | 149 | µstrain/°C |
| Thermal shock resistance | 239 | – | 325 | °C |
| Thermal distortion resistance | 0.00158 | – | 0.00173 | MW/m |
PA6 Molding and Extrusion Electrical properties
| Electrical resistivity | 3.67e19 | – | 9.17e20 | µohm.cm |
| Electrical conductivity | 1.88e-19 | – | 4.7e-18 | %IACS |
| Dielectric constant (relative permittivity) | 12.1 | – | 17.1 | |
| Dissipation factor (dielectric loss tangent) | 0.0722 | – | 0.19 | |
| Dielectric strength (dielectric breakdown) | 24.1 | – | 41 | MV/m |
| Comparative tracking index | 600 | V |
PA6 Molding and Extrusion Magnetic properties
| Magnetic type | Non-magnetic |
PA6 Molding and Extrusion Optical, aesthetic and acoustic properties
| Refractive index | 1.56 | – | 1.57 | |
| Transparency | Translucent | |||
| Acoustic velocity | 908 | – | 1020 | m/s |
| Mechanical loss coefficient (tan delta) | 0.0273 | – | 0.0302 | |
PA6 Molding and Extrusion Absorption & permeability
| Water absorption @ 24 hrs | 1.9 | – | 3.1 | % |
| Water absorption @ sat | 8.2 | – | 11 | % |
| Humidity absorption @ sat | 2.3 | – | 3.2 | % |
| Water vapor transmission | 0.958 | – | 1.73 | g.mm/m².day |
| Permeability (O2) | 0.622 | – | 1.15 | cm³.mm/m².day.atm |
PA6 Molding and Extrusion Processing properties
| Polymer injection molding | Excellent |
| Polymer extrusion | Acceptable |
| Polymer thermoforming | Limited use |
| Linear mold shrinkage | 0.3 – 1.5 % |
| Melt temperature | 227 – 288 °C |
| Mold temperature | 40 – 80 °C |
| Molding pressure range | 68.8 – 138 MPa |
PA6 Molding and Extrusion Durability
| Water (fresh) | Excellent |
| Water (salt) | Excellent |
| Weak acids | Unacceptable |
| Strong acids | Unacceptable |
| Weak alkalis | Limited use |
| Strong alkalis | Limited use |
| Organic solvents | Acceptable |
| Oxidation at 500C | Unacceptable |
| UV radiation (sunlight) | Fair |
| Flammability | Slow-burning |