EN GJS 800-2 hardened & tempered, nodular graphite, Mechanical Properties |
---|
Young’s modulus 168 – 176 GPa |
Flexural modulus * 168 – 176 GPa |
Shear modulus 65 – 70 GPa |
Bulk modulus 121 – 134 GPa |
Poisson’s ratio 0.27 – 0.28 |
Shape factor 18 |
Yield strength (elastic limit) 630 – 710 MPa |
Tensile strength 800 – 900 MPa |
Compressive strength * 639 – 719 MPa |
Flexural strength (modulus of rupture) 630 – 710 MPa |
Elongation 2 – 7 % strain |
Hardness – Vickers 260 – 295 HV |
Fatigue strength at 10^7 cycles 304 – 317 MPa |
Fatigue strength model (stress range) 206 – 250 MPa Parameters: Stress Ratio = 0, Number of Cycles = 1e7 |
Fracture toughness 22 – 34 MPa.m^0.5 |
Mechanical loss coefficient (tan delta) * 6e-4 – 8e-4 |
*Values are approximations. This information’s accuracy is not guaranteed. |