PARA Unfilled Grade Material Data Sheet

PARA Unfilled Grade (Polyarylamide) Material Data Sheet

PARA Unfilled Grade Overview

PARA unfilled grade is a grade of polyarylamide (PARA), designated Polyarylamide. This PARA unfilled grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.

PARA Unfilled Grade Designation

Polyarylamide
TradenamesIxef, Nylon-MXD6

PARA Unfilled Grade Typical uses

Automotive, blow molding applications, films (bi-axially oriented, cast, mulatilayer), food applications, monofilaments, packaging, piping, sheet, tubing

PARA Unfilled Grade Composition detail

Polymer100  %

PARA Unfilled Grade Physical properties

Density1.12–1.22g/cm3

PARA Unfilled Grade Mechanical properties

Young’s modulus4.4–4.7GPa
Specific stiffness3.69–4.1MN.m/kg
Yield strength (elastic limit)69.4–83.9MPa
Tensile strength83–99MPa
Specific strength58.9–72.4kN.m/kg
Elongation2–2.3% strain
Elongation at yield2.82–4.06% strain
Compressive modulus4.33–4.77GPa
Compressive strength98.9–120MPa
Flexural modulus4.4–4.5GPa
Flexural strength (modulus of rupture)157–160MPa
Shear modulus1.57–1.74GPa
Shear strength49.4–59.8MPa
Bulk modulus4.33–4.77GPa
Poisson’s ratio0.368–0.383 
Shape factor5.9
Hardness – Vickers21–24HV
Hardness – Rockwell M107–108 
Hardness – Rockwell R120–140 
Hardness – Shore D79–92 
Elastic stored energy (springs)533–769kJ/m3
Fatigue strength at 10^7 cycles33–39.9MPa

PARA Unfilled Grade Impact & fracture properties

Fracture toughness4.22–5.11MPa.m0.5
Toughness (G)3.94–5.71kJ/m2
Impact strength, notched 23 °C1.9–2kJ/m2

PARA Unfilled Grade Thermal properties

Melting point229–245°C
Glass temperature75–92°C
Heat deflection temperature 0.45MPa145–151°C
Heat deflection temperature 1.8MPa82  °C
Maximum service temperature230–239°C
Minimum service temperature-25  °C
Thermal conductivity0.43–0.47W/m.°C
Specific heat capacity1560–1630J/kg.°C
Thermal expansion coefficient50–72µstrain/°C
Thermal shock resistance228–343°C
Thermal distortion resistance0.00622–0.00903MW/m

PARA Unfilled Grade Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)3.5

PARA Unfilled Grade Magnetic properties

Magnetic typeNon-magnetic

PARA Unfilled Grade Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1920–2029m/s
Mechanical loss coefficient (tan delta)0.0103–0.0149 

PARA Unfilled Grade Absorption & permeability

Water absorption @ 24 hrs0.31–5.8%
Water absorption @ sat5.8  %

PARA Unfilled Grade Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use

PARA Unfilled Grade Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsLimited use
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySlow-burning