Designation: CuMn13Al9
Mechanical properties: Bronze CuMn13Al9 Mechanical Properties (cast, aluminum bronze)
| Young’s modulus | 119 | – | 122 | GPa |
| Specific stiffness | 15.6 | – | 16.6 | MN.m/kg |
| Yield strength (elastic limit) | 380 | – | 470 | MPa |
| Tensile strength | 740 | – | 820 | MPa |
| Specific strength | 50.5 | – | 62.9 | kN.m/kg |
| Elongation | 9 | – | 20 | % strain |
| Compressive strength | 380 | – | 470 | MPa |
| Flexural modulus | 119 | – | 122 | GPa |
| Flexural strength (modulus of rupture) | 380 | – | 470 | MPa |
| Shear modulus | 44 | – | 45.1 | GPa |
| Bulk modulus | 129 | – | 132 | GPa |
| Poisson’s ratio | 0.34 | – | 0.35 | |
| Shape factor | 21 | |||
| Hardness – Vickers | 200 | – | 260 | HV |
| Elastic stored energy (springs) | 605 | – | 908 | kJ/m^3 |
| Fatigue strength at 10^7 cycles | 264 | – | 282 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 241 | – | 309 | MPa |
Impact & fracture properties: Bronze CuMn13Al9 Mechanical Properties (cast, aluminum bronze)
| Fracture toughness | 30.6 | – | 35.8 | MPa.m^0.5 |
| Toughness (G) | 7.81 | – | 10.6 | kJ/m^2 |
MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey