Aluminum 6061 T42 Mechanical Properties

Designation
6061, wrought
ConditionT42 (Solution heat-treated and naturally aged to a substantially stable condition)
UNS numberA96061
EN nameEN AW-6061 (EN AW-Al Mg1SiCu)
EN number3.3211

Aluminum 6061 T42 Mechanical Properties

Young’s modulus66.6–70GPa
Specific stiffness24.5–25.8MN.m/kg
Yield strength (elastic limit)92.6–108MPa
Tensile strength206–240MPa
Specific strength34.1–39.8kN.m/kg
Elongation16–23% strain
Compressive modulus67.9–71.3GPa
Compressive strength92.6–108MPa
Flexural modulus66.6–70GPa
Flexural strength (modulus of rupture)92.6–108MPa
Shear modulus25.6–26.9GPa
Bulk modulus66.6–70GPa
Poisson’s ratio0.325–0.335 
Shape factor39.6   
Hardness – Vickers87–108HV
Elastic stored energy (springs)63–85.1kJ/m^3
Fatigue strength at 10^7 cycles91.1–106MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles83.1–116MPa

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey